PVD (Physical Vapor Deposition) film layer preparation method for improving chromatic aberration of front side of interference color

By setting an appropriate distance and external magnetic field in the coating equipment to change the particle trajectory, the problem of positive side color difference of the interference film layer is solved, and better color consistency of the film layer is achieved.

CN118895484APending Publication Date: 2024-11-05SHENZHEN SENFUNG VACUUM PLATING
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411073416.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In ordinary coating processes, there is a problem of opposite-sided color on the front side, which leads to color characterization being affected by film thickness. The color difference of complex film layers is large, and the existing improvement measures are limited in effect.

Method used

By setting the target material to the goods at an appropriate distance and attaching an external magnetic field to the coating equipment, the particle movement trajectory is changed, and the number of particles around the sides of the goods increases, thereby improving the color difference between the front and side.

Benefits of technology

The positive side color difference of the interference film layer is effectively reduced and the color consistency of the film layer is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895484A_ABST
    Figure CN118895484A_ABST
Patent Text Reader

Abstract

The invention discloses a PVD (Physical Vapor Deposition) film layer preparation method for improving interference color front-side chromatic aberration, and belongs to the field of PVD film coating. Comprising the following steps: S1, putting a substrate material into a coating chamber, and heating and vacuumizing; s2, argon is introduced, a bias power supply is turned on, and arc light cleaning is carried out; s3, turning on an external magnetic field power supply, turning on two pairs of Cr targets, and depositing a pure Cr layer; s4, two pairs of Si targets are started, N2 is introduced, and a CrSiN layer is deposited; s5, gas C2H2 is introduced, and a CrSiCN layer is deposited; s6, closing the pair of Cr targets and the pair of Si targets, adjusting the current of the Cr targets and the Si targets, and depositing a CrSiCN layer of the interference film layer; s7, closing the Cr and Si targets, opening the other pair of Cr targets, closing the gas N2, and depositing an interference film CrC layer; and S8, the Cr target is closed, the Si target is opened, an interference film layer SiC layer is deposited, and film coating is finished. A proper distance is set between the target material and the goods, and an external magnetic field is added to change the moving track of particles in a furnace, so that the particles wound and plated on the side surfaces of the goods are increased, and the color difference between the front surfaces and the side surfaces of the goods is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PVD coating, and in particular relates to a method for preparing a PVD film layer for improving the positive-side chromatic aberration of interference colors. Background Art

[0002] In common coating processes, interference films have the problem of different colors on the front side. The main reason for this problem is that the sputtering time of the front target is longer than that of the side, which makes the thickness of the front film much greater than that of the side film. Interference colors interfere with each other through multiple film layers, and their color representation is affected by the film thickness. Therefore, the more complex the film layer, the greater the difference in color on the front side. The usual improvement measures are to use a three-dimensional rotating rack, increase the rotating rack speed, reduce the current, etc. to improve the difference in color on the front side. However, each of the above measures has a limited improvement on the color difference on the front side, and none of them can completely overcome the problem of different colors on the front side. Summary of the invention

[0003] In order to solve the above problems, the purpose of the present invention is to provide a PVD film preparation method for improving the chromatic aberration of the front side of the interference color, by setting the target material and the goods at an appropriate distance, and adding an external magnetic field at the same time, changing the trajectory of the particles in the furnace, so that the number of particles plated around the side of the goods increases, thereby improving the chromatic aberration of the front and side of the goods.

[0004] To achieve the above object, the technical solution of the present invention is as follows:

[0005] The present invention provides a PVD film preparation method for improving the positive side chromatic aberration of interference colors, comprising the steps of:

[0006] S1: Clean the substrate material, put the cleaned substrate material into the coating chamber, and heat and evacuate the coating chamber;

[0007] S2: When the background vacuum of the coating chamber reaches 0.001Pa, argon gas is introduced to make the gas pressure reach the preset value, and the bias power supply is turned on to perform arc cleaning;

[0008] S3: Adjust the Ar gas intake to make the gas pressure reach a specific value, adjust the bias voltage, turn on the external magnetic field power supply, turn on two pairs of Cr targets, and deposit a pure Cr layer;

[0009] S4: Turn on two pairs of Si targets, introduce N2, adjust the bias voltage, and deposit the CrSiN layer;

[0010] S5: introducing C2H2 gas to deposit a CrSiCN layer;

[0011] S6: close a pair of Cr targets and a pair of Si targets, adjust the current of the Cr target and the Si target, adjust the flow rate of N2 and C2H2, and deposit the CrSiCN layer of the interference film layer;

[0012] S7: turn off the Cr and Si targets, turn on another pair of Cr targets, turn off the gas N2, adjust the flow rate of the gas C2H2, and deposit the interference film layer CrC layer;

[0013] S8: Turn off the Cr target, turn on the Si target, adjust the flow rate of C2H2 gas, deposit the interference film SiC layer, end the coating, and turn off the external magnetic field power supply.

[0014] Furthermore, in the present method, the target configuration includes two pairs of Si targets and two pairs of Cr targets, and the targets are all placed outside the turntable, wherein the two pairs of Si targets are placed on the same side of the device, and the two pairs of Cr targets are placed on the other side, forming four coil magnetic fields and five Cr arcs.

[0015] Furthermore, in steps S3-S8, the current of the external magnetic field is set to 7A, and the distance between the target and the base material is 90mm. By setting an appropriate distance between the target and the base material (coated article) and simultaneously applying an external magnetic field, the trajectory of the particles in the furnace is changed, so that more particles are plated around the side of the product, thereby improving the color difference between the front and side of the product.

[0016] Furthermore, in step S1, the cleaning method is ultrasonic cleaning, which can remove dirt, fingerprints and other problems of the incoming base material and ensure the cleanliness of the base material before magnetron sputtering.

[0017] Furthermore, in step S1, the insulation temperature after heating is 200°C.

[0018] Further, in step S2, the predetermined value of the gas pressure is 0.2 Pa, the bias voltage is set to -300 V, and the arc cleaning time is 1 minute.

[0019] Furthermore, in step S3, the specific value of the gas pressure is 0.3 Pa, the bias voltage is adjusted to -200 V, the current of the Cr target is set to 20 A, and the deposition time of the pure Cr layer is 15 minutes.

[0020] Furthermore, in step S4, the Si target current is set to 10 A, the flow rate of N2 is set to 70 sccm, the bias voltage is adjusted to -150 V, and the deposition time of the CrSiN layer is 50 minutes.

[0021] Furthermore, in step S5, the C2H2 flow rate is set to 5 sccm, and the deposition time of the CrSiCN layer is 60 minutes.

[0022] Furthermore, in step S6, the Cr target current is adjusted to 2 A, the Si target current is adjusted to 10 A, the gas N2 flow rate is adjusted to 120 sccm and the C2H2 flow rate is adjusted to 25 sccm, and the deposition time of the CrSiCN layer is adjusted to 100 minutes.

[0023] Furthermore, in step S7, the current of the Cr target is set to 10 A, the flow rate of C2H2 is set to 10 sccm, and the deposition time of the CrC layer is 15 minutes.

[0024] Furthermore, in step S8, the current of the Si target is set to 10 A, the flow rate of C2H2 is set to 10 sccm, and the deposition time of the SiC layer is 15 minutes.

[0025] Compared with the prior art, the beneficial effect of the present invention is that by setting the target material and the goods at an appropriate distance and adding an external magnetic field at the same time, the trajectory of the particles in the furnace is changed, so that more particles are plated around the side of the goods, thereby improving the color difference between the front and side of the goods. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a flowchart of the preparation method of this embodiment.

[0027] Figure 2 It is a top view of a conventional coating device in the prior art.

[0028] Figure 3 It is a top view of the coating equipment with an external magnetic field added in this embodiment.

[0029] Figure 4 It is a schematic diagram of the magnetic field of the coating equipment in the prior art.

[0030] Figure 5 Schematic diagram of the magnetic field of the membrane device with an external magnetic field added in this embodiment. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0032] To achieve the above object, the technical solution of the present invention is as follows:

[0033] See also Figure 1 As shown, this embodiment provides a PVD film preparation method for improving the positive side chromatic aberration of interference colors. The equipment configuration is as follows: including two pairs of Si targets and two pairs of Cr targets. The target materials are placed on the outside of the rotating frame (i.e., the furnace wall), wherein the two pairs of Si targets are placed on the same side of the equipment, and the two pairs of Cr targets are placed on the other side, four coil magnetic fields, and five Cr arcs. The coating method includes the following steps:

[0034] S1: Clean the substrate material, put the cleaned substrate material into the coating chamber, and heat and evacuate the coating chamber;

[0035] S2: When the background vacuum of the coating chamber reaches 0.001Pa, argon gas is introduced to make the gas pressure reach the preset value, and the bias power supply is turned on to perform arc cleaning;

[0036] S3: Adjust the Ar gas intake to make the gas pressure reach a specific value, adjust the bias voltage, turn on the external magnetic field power supply, turn on two pairs of Cr targets, and deposit a pure Cr layer;

[0037] S4: Turn on two pairs of Si targets, introduce N2, adjust the bias voltage, and deposit the CrSiN layer;

[0038] S5: introducing C2H2 gas to deposit a CrSiCN layer;

[0039] S6: close a pair of Cr targets and a pair of Si targets, adjust the current of the Cr target and the Si target, adjust the flow rate of N2 and C2H2, and deposit the CrSiCN layer of the interference film layer;

[0040] S7: turn off the Cr and Si targets, turn on another pair of Cr targets, turn off the gas N2, adjust the flow rate of the gas C2H2, and deposit the interference film layer CrC layer;

[0041] S8: Turn off the Cr target, turn on the Si target, adjust the flow rate of C2H2 gas, deposit the interference film SiC layer, end the coating, and turn off the external magnetic field power supply.

[0042] Furthermore, in the present method, the target configuration includes two pairs of Si targets and two pairs of Cr targets, and the targets are all placed outside the turntable, wherein the two pairs of Si targets are placed on the same side of the device, and the two pairs of Cr targets are placed on the other side, forming four coil magnetic fields and five Cr arcs.

[0043] Furthermore, in step S1, the cleaning method is ultrasonic cleaning, which can remove dirt, fingerprints and other problems of the incoming base material and ensure the cleanliness of the base material before magnetron sputtering.

[0044] Furthermore, in step S1, the insulation temperature after heating is 200°C.

[0045] Further, in step S2, the predetermined value of the gas pressure is 0.2 Pa, the bias voltage is set to -300 V, and the arc cleaning time is 1 minute.

[0046] Furthermore, in step S3, the specific value of the gas pressure is 0.3 Pa, the bias voltage is adjusted to -200 V, the current of the Cr target is set to 20 A, and the deposition time of the pure Cr layer is 15 minutes.

[0047] Furthermore, in step S4, the Si target current is set to 10 A, the flow rate of N2 is set to 70 sccm, the bias voltage is adjusted to -150 V, and the deposition time of the CrSiN layer is 50 minutes.

[0048] Furthermore, in step S5, the C2H2 flow rate is set to 5 sccm, and the deposition time of the CrSiCN layer is 60 minutes.

[0049] Furthermore, in step S6, the Cr target current is adjusted to 2 A, the Si target current is adjusted to 10 A, the gas N2 flow rate is adjusted to 120 sccm and the C2H2 flow rate is adjusted to 25 sccm, and the deposition time of the CrSiCN layer is adjusted to 100 minutes.

[0050] Furthermore, in step S7, the current of the Cr target is set to 10 A, the flow rate of C2H2 is set to 10 sccm, and the deposition time of the CrC layer is 15 minutes.

[0051] Furthermore, in step S8, the current of the Si target is set to 10 A, the flow rate of C2H2 is set to 10 sccm, and the deposition time of the SiC layer is 15 minutes.

[0052] In this embodiment, by setting the target material and the goods at an appropriate distance, and adding an external magnetic field to the device, see Figure 3 , 5 After superimposing the external magnetic field, the magnetic field trajectory can be changed. Through debugging, the optimal current size can be obtained, and the particle running trajectory in the furnace can be changed, so that more particles are plated around the side of the goods, thereby improving the color difference between the front and side of the goods.

[0053] In this embodiment, after the coating is completed, through measurement, the color values ​​of the Lab color model of the front color of the base material are: L: 54, a: 5, b: -14.

[0054] At the same time, by controlling the variables, adjusting the target-substrate distance (the distance between the target material and the substrate material) and the current of the external magnetic field, the color value of the side color of the coating was measured, and the results are shown in Tables 1 and 2. Table 1 shows the color value of the side color when the current of the external magnetic field is set to 7A and different target-substrate distances are set; Table 2 shows the color value of the side color when the target-substrate distance is 90mm and different external magnetic field currents are set.

[0055] Table 1:

[0056] DOE Target-substrate distance / mm L a b result 1 50 58.97 0.63 -1.73 Difference 2 60 56.21 0.58 -2.31 Poor 3 70 58.28 0.15 -3.61 Poor 4 80 53.89 0.53 -4.0 Poor 5 90 52.29 1.03 -4.7 optimal 6 100 52.89 0.73 -3.54 Poor

[0057] Table 2:

[0058] DOE Current / A result L a b 1 4 Difference 53.26 0.98 -4.3 2 5 Poor 53.13 1.34 -4.6 3 6 Poor 53.59 1.65 -5.8 4 7 optimal 54.39 1.83 -7.4 5 8 Poor 53.67 1.46 -6.1 6 10 Poor 52.73 1.04 -5.2

[0059] From the results in Table 1 and Table 2, it can be seen that in steps S3-S8, when the current of the external magnetic field is set to 7A and the distance between the target material and the base material is 90mm, the color difference between the front and side of the product is the smallest and the effect is the best.

[0060] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference color, characterized in that: Includes steps: S1: Clean the substrate material, put the cleaned substrate material into the coating chamber, and heat and evacuate the coating chamber; S2: When the background vacuum of the coating chamber reaches 0.001Pa, argon gas is introduced to make the gas pressure reach the preset value, and the bias power supply is turned on to perform arc cleaning; S3: Adjust the Ar gas intake to make the gas pressure reach a specific value, adjust the bias voltage, turn on the external magnetic field power supply, turn on two pairs of Cr targets, and deposit a pure Cr layer; S4: Turn on two pairs of Si targets, introduce N2, adjust the bias voltage, and deposit the CrSiN layer; S5: introducing C2H2 gas to deposit a CrSiCN layer; S6: close a pair of Cr targets and a pair of Si targets, adjust the current of the Cr target and the Si target, adjust the flow rate of N2 and C2H2, and deposit the CrSiCN layer of the interference film layer; S7: turn off the Cr and Si targets, turn on another pair of Cr targets, turn off the gas N2, adjust the flow rate of the gas C2H2, and deposit the interference film layer CrC layer; S8: Turn off the Cr target, turn on the Si target, adjust the flow rate of C2H2 gas, deposit the interference film SiC layer, end the coating, and turn off the external magnetic field power supply.

2. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference color according to claim 1, characterized in that: In steps S3-S8, the current of the external magnetic field is set to 7A, and the distance between the target material and the substrate material is 90 mm.

3. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference color according to claim 1, characterized in that: In step S1, the holding temperature after heating is 200°C.

4. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference color according to claim 1, characterized in that: In step S2, the predetermined value of the gas pressure is 0.2 Pa, the bias voltage is set to -300 V, and the arc cleaning time is 1 minute.

5. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference color according to claim 1, characterized in that: In step S3 , the specific value of the gas pressure is 0.3 Pa, the bias voltage is adjusted to −200 V, the current of the Cr target is set to 20 A, and the deposition time of the pure Cr layer is 15 minutes.

6. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference color according to claim 1, characterized in that: In step S4, the Si target current is set to 10 A, the flow rate of N2 is set to 70 sccm, the bias voltage is adjusted to -150 V, and the deposition time of the CrSiN layer is 50 minutes.

7. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference colors as claimed in claim 1, characterized in that: In step S5, the C2H2 flow rate is set to 5 sccm, and the deposition time of the CrSiCN layer is 60 minutes.

8. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference colors as claimed in claim 1, characterized in that: In step S6, the Cr target current is adjusted to 2A, the Si target current is adjusted to 10A, the gas N2 flow rate is adjusted to 120sccm and the C2H2 flow rate is adjusted to 25sccm, and the deposition time of the CrSiCN layer is adjusted to 100 minutes.

9. A method for preparing a PVD film layer for improving the positive side chromatic aberration of interference colors as claimed in claim 1, characterized in that: In step S7, the current of the Cr target is set to 10 A, the flow rate of C2H2 is set to 10 sccm, and the deposition time of the CrC layer is 15 minutes.

10. The method for preparing a PVD film layer for improving the positive side chromatic aberration of interference color according to claim 1, characterized in that: In step S8, the current of the Si target is set to 10A, the flow rate of C2H2 is set to 10sccm, and the deposition time of the SiC layer is 15 minutes.

Citation Information

Cited By

  • Coated product and manufacturing method and application thereof

    CN116590654A

  • Coated products, their manufacturing methods and applications