Stabilized preparation method of high-entropy monatomic catalyst, catalyst and application

Through wet ball milling and freeze-drying combined with fast Joule heat method, the preparation process of high-entropy single-atom catalysts is simplified, and the problems of long time, complex equipment and high cost in the existing technology are solved, and efficient and low-cost catalyst preparation is achieved. and performance improvement.

CN118895524AActive Publication Date: 2024-11-05UESTC (SHENZHEN) ADVANCED RES INST
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410936136.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The existing high-entropy single-atom catalyst preparation methods have problems such as long time, complex equipment, metal agglomeration, limited material selection and high cost, resulting in low production efficiency, high cost and unstable catalyst performance.

Method used

Wet ball milling and freeze-drying combined with fast Joule heat method are used to prepare high-entropy single atom catalyst through ball mill and flash heat equipment, avoiding long-term high-temperature treatment, simplifying the process flow, and using simple equipment to ensure uniform dispersion of metal atoms. and catalyst stability.

Benefits of technology

It realizes efficient and low-cost high-entropy single-atom catalyst preparation, improves the performance and stability of the catalyst, broadens its application range, and reduces production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895524A_ABST
    Figure CN118895524A_ABST
Patent Text Reader

Abstract

The invention provides a stable preparation method of a high-entropy monatomic catalyst, which comprises the following steps: uniformly mixing metal salt and a load substrate by using wet ball milling to prepare mixed slurry; freeze-drying the mixed slurry to obtain dry powder; and treating the dry powder by adopting a rapid Joule thermal method to prepare the high-entropy monatomic catalyst. Wherein the metal salt comprises any one of nitrate, sulfate or acetate; the load substrate comprises graphene, carbon nanotubes, carbon black, glucose, melamine or urea, and cerium oxide, silicon oxide or aluminum oxide. The preparation method is simple in process, high in efficiency and low in production cost, only a ball mill and flash heating equipment are needed in the preparation process, a large number of solvents and chemical reagents are not needed, and environment friendliness is achieved. Wet ball milling is combined with freeze drying, agglomeration is prevented, uniformity is kept, the prepared high-entropy monatomic catalyst is uniform in molecular morphological structure, more active sites can be exposed, and catalytic performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts for preparing new energy batteries, and in particular to a stabilization preparation method of a high-entropy single-atom catalyst, a catalyst and an application thereof. Background Art

[0002] High entropy single atoms refer to the introduction of the concept of high entropy in single-atom catalysts, through a variety of (usually five or more) different metal elements, in the form of nearly equimolar ratios, distributed at the nanoscale or atomic level. These single atoms are evenly dispersed on the supporting material (such as carbon-based materials, oxides, etc.), providing unique electronic structure and catalytic performance through the high entropy effect. In the process of preparing high entropy single-atom catalysts, the existing technical solutions mainly use wet chemical methods, chemical vapor deposition (CVD), atomic layer deposition (ALD) and other methods.

[0003] However, the above traditional methods have the following problems:

[0004] Long time: Traditional heat treatment methods usually take several hours or even longer to complete. This not only reduces production efficiency, but also increases energy consumption, leading to higher production costs.

[0005] Complex equipment: Traditional methods usually require complex multi-step processing procedures and expensive equipment, which increases the complexity and cost of the preparation process. For example, CVD and ALD methods require precise control of gas flow and reaction environment, which are difficult to operate.

[0006] Metal agglomeration: Long-term high-temperature treatment easily causes metal atoms to agglomerate on the surface of the support material to form nanoparticles. This not only reduces the active sites of the single-atom catalyst, but also reduces the performance and stability of the catalyst.

[0007] Limited material selection: Existing methods have limited choices for supporting materials and are difficult to adapt to the needs of different catalytic reactions. In particular, when dealing with carbon-based materials, the compatibility and effect of traditional methods are poor.

[0008] High cost: Long processing time and complicated process flow increase production cost.

[0009] Therefore, there is an urgent need for a fast and low-cost method to prepare high-entropy single-atom catalysts. Summary of the invention

[0010] In view of the deficiencies in the prior art, the present invention proposes a method for preparing a high entropy single atom catalyst to overcome the deficiencies in the prior art.

[0011] The technical solution adopted by the present invention is as follows:

[0012] In a first aspect, a method for preparing a stabilized high entropy single-atom catalyst is provided, comprising the following steps: mixing a metal salt and a support substrate by wet ball milling to prepare a mixed slurry;

[0013] The mixed slurry is freeze-dried to obtain a dry powder;

[0014] The dry powder was treated by rapid Joule heating to prepare high entropy single atom catalyst.

[0015] Further, the metal salt includes any one of the following three:

[0016] Nitrates: iron (III) nitrate (Fe(NO3)3), nickel (II) nitrate (Ni(NO3)2), cobalt (II) nitrate (Co(NO3)2), copper (II) nitrate (Cu(NO3)2), manganese (II) nitrate (Mn(NO3)2), palladium (II) nitrate (Pd(NO3)2), platinum (IV) nitrate (Pt(NO3)4);

[0017] Sulfates: iron (II) sulfate (FeSO4), nickel (II) sulfate (NiSO4), cobalt (II) sulfate (CoSO4), copper (II) sulfate (CuSO4), manganese (II) sulfate (MnSO4), platinum (IV) sulfate (PtSO4), palladium (II) sulfate (PdSO4);

[0018] Acetates: Iron (III) acetate (Fe(C2H3O2)3), Nickel (II) acetate (Ni(C2H3O2)3), Cobalt (II) acetate (Co(C2H3O2)3), Copper (II) acetate (Cu(C2H3O2)3), Manganese (II) acetate (Mn(C2H3O2)3), Palladium (II) acetate (Pd(C2H3O2)3), Platinum (IV) acetate (Pt(C2H3O2)3).

[0019] Furthermore, the load substrate includes a carbon substrate, and the carbon substrate includes graphene, carbon nanotubes, carbon black, glucose, melamine or urea.

[0020] Furthermore, the support substrate comprises a metal oxide substrate, and the metal oxide substrate comprises cerium oxide, silicon oxide or aluminum oxide.

[0021] Furthermore, the wet ball milling includes: mixing the load substrate and the metal salt evenly, adding anhydrous ethanol and ammonia water to form a uniform mixed solution; adding the mixed solution to a ball mill, setting the ball mill speed to 300-500rpm, and the room temperature ball milling time to 6-12h; and further low temperature ball milling for 3-4h under an inert atmosphere.

[0022] Furthermore, the freeze drying includes: freezing the mixed slurry, the freezing temperature is -4°C, the freezing time is 4 hours, and the mixed slurry is completely frozen; starting the freeze dryer, setting the vacuum degree to 10Pa, the sublimation temperature to -20°C, and the sublimation time to 2 hours.

[0023] Furthermore, the rapid Joule heating method includes: opening the vacuum box of the flash heating equipment, placing the dry powder on the heating material, closing the vacuum box of the flash heating equipment, evacuating the box and then introducing an inert gas, and performing rapid Joule heating treatment on the dry powder at a predetermined voltage, current, time, and number of times.

[0024] Furthermore, the electrode voltage is preset to 15-40V; the electrode current is preset to 15-80A; the time is preset to 0.5-2s; one heating cycle is 1.5-4s; and the number of heating times is preset to 5-10 times.

[0025] In a second aspect, a high entropy single-atom catalyst is provided, which is prepared according to the preparation method provided in the first aspect.

[0026] Secondly, a high entropy single-atom catalyst is provided for use in water electrolysis, fuel cells and metal-air batteries.

[0027] It can be seen from the above technical solution that the beneficial technical effects of the present invention are as follows:

[0028] 1. The preparation method has simple process, high efficiency and low production cost: only ball mill and flash heating equipment are needed in the preparation process, without large amount of solvents and chemical reagents, which is environmentally friendly.

[0029] 2. Wet ball milling combined with freeze drying is used to prevent agglomeration and maintain uniformity. The prepared high-entropy single-atom catalyst has a uniform molecular morphology and structure, which helps to expose more active sites and improve catalytic performance.

[0030] 3. The prepared catalyst has good stability and can be applied to a variety of carbon-based materials and other high-temperature resistant materials, broadening the application range of high-entropy single-atom catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the prior art description. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0032] Figure 1 is a flow chart of the preparation method of an embodiment of the present invention;

[0033] Figure 2This is a temperature-time curve of the rapid Joule heat treatment process of Experiment 1 of the embodiment of the present invention;

[0034] Figure 3 A physical picture of a high entropy single atom catalyst prepared in Experiment 1 of an embodiment of the present invention;

[0035] Figure 4 This is a graph of electrochemical test data for the oxygen evolution reaction of a high entropy single-atom catalyst prepared in Experiment 1 of an embodiment of the present invention. DETAILED DESCRIPTION

[0036] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.

[0037] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the present invention belongs.

[0038] Example

[0039] In order to facilitate the technical personnel to understand the creativity of the technical solution of this application, the concepts of single-atom metal, high-entropy single-atom metal and high-entropy alloy are briefly explained first:

[0040] Monatomic metal: usually refers to the existence of metal elements in the form of single atoms, and only involves one metal element.

[0041] High-entropy single-atom metals: High-entropy single atoms are composed of a variety of different metal atoms, each of which exists in the form of isolated single atoms. In terms of structure, single metal atoms are evenly dispersed on the substrate material (usually a carbon substrate), and each metal atom is isolated and distributed without forming clusters or alloy phases.

[0042] High entropy alloy: It is composed of at least five elements in equal or approximately equal molar ratios, and these elements are evenly distributed in the crystal lattice. In terms of structure, multiple metal elements are randomly distributed in the crystal lattice to form a solid solution structure or intermetallic compound, which has a higher configuration entropy than traditional alloys.

[0043] The inventors of this application have found that in the field of catalysts, high entropy alloys show good stability and activity in some catalytic reactions, but are not as precise as high entropy single-atom materials. For high entropy single-atom catalysts, because they involve the uniform dispersion and synergistic effect of multiple metal elements, the preparation process is more complicated, and it is necessary to solve the problem of uniform dispersion of each metal element under rapid high-temperature treatment, as well as the stability of different metal elements on the carbon substrate.

[0044] This embodiment provides a method for stabilizing and preparing a high-entropy single-atom electrocatalyst, and the materials required mainly include a metal precursor and a loading substrate.

[0045] In a specific embodiment, the metal precursor can be selected from any one of the following three metal salts:

[0046] Nitrates: Iron (III) nitrate (Fe(NO3)3), Nickel (II) nitrate (Ni(NO3)2), Cobalt (II) nitrate (Co(NO3)2), Copper (II) nitrate (Cu(NO3)2), Manganese (II) nitrate (Mn(NO3)2), Palladium (II) nitrate (Pd(NO3)2), Platinum (IV) nitrate (Pt(NO3)4).

[0047] Sulfates: Iron(II) sulfate (FeSO4), Nickel(II) sulfate (NiSO4), Cobalt(II) sulfate (CoSO4), Copper(II) sulfate (CuSO4), Manganese(II) sulfate (MnSO4), Platinum(IV) sulfate (PtSO4), Palladium(II) sulfate (PdSO4).

[0048] Acetates: Iron (III) acetate (Fe(C2H3O2)3), Nickel (II) acetate (Ni(C2H3O2)3), Cobalt (II) acetate (Co(C2H3O2)3), Copper (II) acetate (Cu(C2H3O2)3), Manganese (II) acetate (Mn(C2H3O2)3), Palladium (II) acetate (Pd(C2H3O2)3), Platinum (IV) acetate (Pt(C2H3O2)3).

[0049] The support substrate includes: a carbon substrate and a metal oxide substrate. In a specific embodiment, the carbon substrate can be selected from: graphene, carbon nanotubes, carbon black, glucose, melamine, urea, etc. The metal oxide can be selected from: cerium oxide (CeO2), silicon oxide (SiO), aluminum oxide (Al2O3), etc.

[0050] When the selected load substrate is a carbon substrate, some carbon substrates need to be pretreated. The pretreatment method is as follows:

[0051] Glucose, sucrose: Through rapid Joule heat treatment, impurities and moisture are removed to obtain high-purity carbon.

[0052] Using the above metal precursors and support substrates, the high entropy single atom electrocatalyst was prepared according to the following steps:

[0053] Step 1: Use wet ball milling to mix the metal salt and the load substrate to prepare a mixed slurry.

[0054] When preparing a precursor in the form of a mixed slurry, the metal salt and the load substrate are preferably mixed by ball milling, and the specific steps are: the weighed load substrate and the metal salt precursor are mixed evenly, and anhydrous ethanol and ammonia water are added according to the weight of the substrate and the precursor to form a uniform mixed solution; the mixed solution is added to a ball mill, and an appropriate amount of grinding media (single silica balls, zirconium oxide balls or their composite media) is added; the ball mill speed is set to 300-500rpm, and the room temperature ball milling time is 6-12h to ensure that the mixture is initially mixed. In an inert atmosphere (preferably argon), further low-temperature ball milling is performed for 3-4h to improve mixing uniformity and particle fineness.

[0055] In this step, the high-energy ball milling and multi-step ball milling treatment described above can be used to obtain a more uniform mixture of carbon source and metal precursor, which is helpful for uniformly generating high-entropy single-atom catalysts during the rapid Joule heat treatment process in the subsequent step; at the same time, it can reduce the energy required for rapid Joule heat treatment, improve preparation efficiency, and reduce costs. Using ammonia water as a surfactant for surface activation treatment can increase the reactivity of the metal precursor and promote uniform dispersion of metal atoms during the rapid Joule heat treatment process in the subsequent step.

[0056] Low-temperature ball milling and composite ball milling media treatment under inert atmosphere protection can effectively control the particle size and morphology of the mixture, which is helpful to generate high-entropy single-atom catalysts with specific structures during the rapid Joule heat treatment process in the subsequent steps.

[0057] Step 2: freeze-dry the mixed slurry to obtain dry powder

[0058] First, the mixed slurry is frozen. In a specific embodiment, the mixed slurry after wet ball milling is poured into a tray of a freeze dryer to ensure that the mixed slurry is evenly distributed. The tray is placed in the freeze dryer, and the freezing temperature is set to -4°C and the freezing time is 4 hours to ensure that the mixed slurry is completely frozen.

[0059] The frozen mixed slurry is then dried, and a freeze dryer is started. In a specific embodiment, the vacuum degree is set to 10 Pa, the sublimation temperature is -20°C, and the sublimation time is 2 hours. After the freeze drying is completed, the dried frozen mixed slurry is taken out of the dryer to obtain a loose dry powder.

[0060] In this step, freeze drying is used, and water is directly sublimated from the solid state to the gaseous state, which avoids the problem of particle agglomeration caused by high temperature drying, making the obtained powder more uniform and loose. The freeze-dried powder has a larger specific surface area, and the uniform dispersion and reaction of metal atoms during the rapid Joule heat treatment process in the subsequent steps improve the activity of the catalyst. At the same time, freeze drying under low temperature and vacuum environment can effectively reduce the introduction of impurities, maintain the purity of the material, and improve the performance of the catalyst. The prepared loose powder structure is conducive to uniform heating during the rapid Joule heat treatment process in the subsequent steps, improves the heat conduction efficiency, and ensures the uniform reaction and generation of the material. At the same time, the powder structure after freeze drying is more stable, which is conducive to maintaining its structural integrity during the rapid Joule heat treatment process in the subsequent steps, avoiding structural collapse, and improving the long-term stability of the catalyst.

[0061] Step 3: Prepare high entropy single atom catalyst by fast Joule heating method on dry powder

[0062] The rapid Joule heating method has the following characteristics:

[0063] Uniform heating: The sample is uniformly heated by electric current, avoiding the temperature gradient problem in traditional heating methods, thereby ensuring the uniformity of the material. Strong controllability: The strong current and heating time can be precisely controlled, thereby achieving precise regulation of the material composition and structure to meet different application requirements. Wide applicability: This method is applicable to a variety of carbon substrates and metal precursors, and can be used to prepare high-entropy single-atom catalysts of various compositions, with wide applicability.

[0064] The specific operation of the rapid Joule heating method is as follows: open the vacuum box of the flash heating equipment, place the dry powder on the heating material, the heating material is not limited and can be carbon cloth, carbon paper, carbon felt, carbon plate, nickel foil, etc., in the embodiment, preferably carbon paper, contact the heating electrode. After closing the vacuum box of the flash heating equipment, evacuate the vacuum box, and then introduce inert gas (preferably argon), repeat the operation 5 times to ensure that the air in the cavity is completely exhausted. Then, the dry powder is subjected to rapid Joule heating treatment according to a predetermined voltage, current, time, and number of times. The electrode voltage is preset to 15-40V; the electrode current is preset to 15-80A; the time is preset to 0.5-2s; one heating cycle is 1.5-4s; the number of heating times is preset to 5-10 times.

[0065] The following specific experiments are used to illustrate the technical solution of this application:

[0066] Test 1

[0067] Urea is used as a carbon source loading substrate, and the metal precursors are iron nitrate, nickel nitrate, copper nitrate, zinc nitrate, and platinum nitrate.

[0068] First, weighed urea (5g) and metal precursors iron nitrate (4.04g), nickel nitrate (2.91g), copper nitrate (2.41g), zinc nitrate (2.97g), and platinum nitrate (4.41g) were mixed with 10mL of anhydrous ethanol and 0.5mL of ammonia water to form a uniform mixed solution; the mixed solution was added to a ball mill, and grinding media was added at a ratio of 25:1 to the ball-to-material ratio. The ball mill speed was set to 300rpm, the room temperature ball milling time was 12h, and the low temperature ball milling was further performed for 3h under an inert atmosphere (argon). After the ball milling was completed, the mixed solution was taken out and poured into the tray of the freeze dryer to ensure that the slurry was evenly distributed. The tray was placed in the freeze dryer, and the freezing temperature was set to -4℃ and the freezing time was 4 hours to ensure that the slurry was completely frozen. Start the freeze dryer, set the vacuum degree to 10Pa, the sublimation temperature to -20℃, and the sublimation time to 2 hours. After freeze drying, the dried sample was taken out of the dryer to obtain a loose dry powder.

[0069] The powder obtained by ball milling is evenly distributed between the conductive electrodes of the flash heating device to ensure good contact between the electrodes. Close the vacuum box, evacuate the vacuum, and then introduce argon gas. Repeat the operation 5 times to ensure that the air in the cavity is completely exhausted. Set the heating parameters: applied voltage is 25V, applied current is 35A, processing time is 500ms, and heating cycle is 1500ms. Repeat the above heating and cooling times 10 times to ensure the uniformity and full reaction of the sample. Figure 2 This is the temperature-time curve of the rapid Joule heat treatment process in Experiment 1.

[0070] After the rapid Joule thermal treatment, the sample was taken out of the vacuum box and properly ground and sieved to obtain a uniform high-entropy single-atom catalyst, such as Figure 3 shown.

[0071] Test 2

[0072] Experiment 2 is basically the same as Experiment 1, except that the carbon source loading substrate is replaced with melamine; the ball mill speed is set to 400 rpm, the room temperature ball milling time is 6 h, and the low temperature ball milling time is 3 h; the voltage applied for rapid Joule thermal treatment is 15 V, the applied current is 15 A, the processing time is 1000 ms, and the heating cycle is 2000 ms.

[0073] Test 3

[0074] Experiment 2 is basically the same as Experiment 1, except that the carbon source loading substrate is replaced with cerium dioxide (CeO2); the ball mill speed is set to 500 rpm, the room temperature ball milling time is 8 hours, and the low temperature ball milling time is 4 hours; the voltage applied for rapid Joule thermal treatment is 40 V, the applied current is 80 A, the processing time is 1500 ms, and the heating cycle is 3000 ms.

[0075] Test 4

[0076] Experiment 2 is basically the same as Experiment 1, except that the ball mill speed is set to 500 rpm, the room temperature ball milling time is 10 h, and the low temperature ball milling time is 4 h; the voltage applied for rapid Joule heat treatment is 30 V, the applied current is 65 A, the processing time is 2000 ms, and the heating cycle is 4000 ms.

[0077] Then, the high entropy single-atom catalyst prepared in the above experiment was subjected to electrochemical testing, as follows: Taking carbon cloth as the supporting electrode as an example, the commercial carbon cloth was ultrasonically cleaned in water and ethanol for a few minutes to remove surface impurities, and then dried in an oven. A certain amount of catalyst powder, an appropriate amount of binder (Nafion) and a solvent (a mixed solvent of ethanol and isopropanol) were mixed and mixed in ultrasound for 30 minutes until a uniform catalyst ink was formed. A certain amount of the homogeneous solution was dropped on the cleaned carbon cloth and naturally air-dried for electrochemical testing. The test results are as follows: Figure 4 As shown: Figure 4 In the figure, the left figure is the linear scanning curve, and the right figure is the Tafel slope; Figure 4 It can be seen that: Tests 1-4 at 50mA cm -2 The corresponding overpotentials at current densities of 275, 273, 275, and 291 mV are respectively, and the corresponding Tafel slopes are 38, 31, 35, and 42 mV dec. -1 From the above experimental data, it can be seen that the prepared high-entropy single-atom catalyst sample has excellent electrocatalytic activity and fast reaction kinetics.

[0078] After the above experiments and tests, it can be seen that the rapid Joule heating method has significant advantages in the preparation of high entropy single atom catalysts:

[0079] (1) The preparation process is simple, with high efficiency and low production cost: The rapid Joule heating process is relatively simple and does not require complex equipment and multi-step processing procedures. The material only needs to be placed between carbon-based electrodes and heated by generating Joule heat through electric current, which is easy to operate. The material can be heated to a high temperature in a very short time (a few seconds or tens of seconds), which significantly shortens the preparation time and improves production efficiency. The preparation process does not require complex and multiple equipment, only ball mills and flash heating equipment are required, which reduces equipment costs and operating difficulties. The preparation process also does not require a large amount of solvents and chemical reagents, which reduces the generation of hazardous waste and is environmentally friendly; this rapid processing method greatly reduces energy consumption and production costs.

[0080] (2) The molecular morphology and structure of the catalyst are uniform: Traditional heating methods easily lead to the agglomeration of metal atoms. The preparation method of the present application can achieve extremely high temperatures (usually exceeding 2000°C) in a short period of time, promote the diffusion and uniform dispersion of metal atoms, and ensure the full mixing of multiple metal elements. Due to the characteristics of rapid heating and cooling, metal atoms experience high temperatures in a short period of time but do not stay in a high temperature state for a long time, which reduces the agglomeration of metal atoms and maintains the dispersed state of single atoms, so that the metal atoms are evenly dispersed on the carbon substrate to form a highly uniform single-atom structure; this uniform dispersion helps to expose more active sites and improve the catalytic performance of the catalyst.

[0081] (3) Good catalyst stability: High-entropy single-atom catalysts are formed in a high-temperature environment, have high thermal stability, and are not prone to structural changes. The uniformly dispersed single-atom structure and high-entropy effect work together to help improve the service life and performance stability of the catalyst in practical applications.

[0082] (4) The catalyst has a wide range of applications: This method is flexible in the selection of supporting materials and can be applied to a variety of carbon-based materials and other high-temperature resistant materials, broadening the application range of high-entropy single-atom catalysts.

[0083] The high-entropy single-atom catalyst prepared in this embodiment can be widely used in scenarios such as water electrolysis, fuel cells and metal-air batteries.

[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. A method for stabilizing and preparing a high entropy single-atom catalyst, characterized in that: The following steps are involved: The metal salt and the support substrate are mixed by wet ball milling to prepare a mixed slurry; The mixed slurry is freeze-dried to obtain a dry powder; The dry powder was treated by rapid Joule heating to prepare high entropy single atom catalyst.

2. The method for preparing a high entropy single-atom catalyst by stabilization according to claim 1, characterized in that: The metal salt includes any one of the following three: Nitrates: iron (III) nitrate (Fe(NO3)3), nickel (II) nitrate (Ni(NO3)2), cobalt (II) nitrate (Co(NO3)2), copper (II) nitrate (Cu(NO3)2), manganese (II) nitrate (Mn(NO3)2), palladium (II) nitrate (Pd(NO3)2), platinum (IV) nitrate (Pt(NO3)4); Sulfates: iron (II) sulfate (FeSO4), nickel (II) sulfate (NiSO4), cobalt (II) sulfate (CoSO4), copper (II) sulfate (CuSO4), manganese (II) sulfate (MnSO4), platinum (IV) sulfate (PtSO4), palladium (II) sulfate (PdSO4); Acetates: Iron (III) acetate (Fe(C2H3O2)3), Nickel (II) acetate (Ni(C2H3O2)3), Cobalt (II) acetate (Co(C2H3O2)3), Copper (II) acetate (Cu(C2H3O2)3), Manganese (II) acetate (Mn(C2H3O2)3), Palladium (II) acetate (Pd(C2H3O2)3), Platinum (IV) acetate (Pt(C2H3O2)3).

3. The method for stabilizing and preparing a high entropy single-atom catalyst according to claim 1, characterized in that: The supporting substrate includes a carbon substrate, and the carbon substrate includes graphene, carbon nanotubes, carbon black, glucose, melamine or urea.

4. The method for stabilizing and preparing a high entropy single-atom catalyst according to claim 1, characterized in that: The supporting substrate includes a metal oxide substrate, and the metal oxide substrate includes cerium oxide, silicon oxide or aluminum oxide.

5. The method for stabilizing and preparing a high entropy single-atom catalyst according to claim 1, characterized in that: The wet ball milling comprises: uniformly mixing the loading substrate and the metal salt, adding anhydrous ethanol and ammonia water to form a uniform mixed solution; adding the mixed solution into a ball milling jar, setting the ball mill speed to 300-500 rpm, and the room temperature ball milling time to 6-12 hours; and further low temperature ball milling for 3-4 hours under an inert atmosphere.

6. The method for stabilizing and preparing a high entropy single-atom catalyst according to claim 1, characterized in that: The freeze drying comprises: freezing the mixed slurry at a freezing temperature of -4°C for 4 hours until the mixed slurry is completely frozen; starting the freeze dryer, setting the vacuum degree to 10 Pa, the sublimation temperature to -20°C, and the sublimation time to 2 hours.

7. The method for stabilizing and preparing a high entropy single-atom catalyst according to claim 1, characterized in that: The rapid Joule heating method comprises: opening the vacuum box of the flash heating equipment, placing the dry powder on the heating material, closing the vacuum box of the flash heating equipment, evacuating the vacuum box and then introducing inert gas, and performing rapid Joule heating treatment on the dry powder according to a predetermined voltage, current, time and number of times.

8. The method for stabilizing and preparing a high entropy single-atom catalyst according to claim 7, characterized in that: The electrode voltage is preset to 15-40V; the electrode current is preset to 15-80A; the time is preset to 0.5-2s; one heating cycle is 1.5-4s; the number of heating times is preset to 5-10 times.

9. A high entropy single atom catalyst, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the high entropy single atom catalyst as claimed in claim 9 in water electrolysis, fuel cells and metal-air batteries.

Citation Information

Patent Citations

  • Method for preparing high-entropy alloy type electrocatalytic oxygen evolution reaction catalyst through high-energy ball milling

    CN110079824A

  • Preparation method of carbon loaded high entropy monatomic catalyst

    CN110773192A

  • Method for synthesizing carbon-supported monatomic catalyst by thermal shock and carbon-supported monatomic catalyst

    CN113151861A

  • Carbon-supported multi-element monatomic metal catalyst

    CN113258088A

  • Non-pyrolytic monatomic alloy catalyst and preparation method thereof

    CN115584523A