Core-shell structure ferroferric oxide-lignin nanosphere as well as preparation method and application thereof

By preparing iron(III) oxide@lignin nanospheres through a stirring-evaporation method in a volatile organic solvent/water binary solvent, the preparation difficulties in the prior art have been solved, and the monodispersity and stability have been improved, making them suitable for applications in advanced optics.

CN118895565AActive Publication Date: 2024-11-05GUANGDONG UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410932521.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Existing technologies are difficult to efficiently prepare monodisperse iron oxide@lignin nanospheres, and iron oxide suffers from poor chemical and colloidal stability during use or long-term storage, requiring cumbersome chemical modification treatments.

Method used

A one-pot method was used to synthesize magnetite with high surface negative charge. Magnetic nanospheres with regular morphology and uniform size were prepared by stirring and evaporation in a volatile organic solvent/water binary solvent. The self-assembly behavior of lignin was used to form a core-shell structure on the surface of magnetite.

Benefits of technology

The efficient and controllable preparation of iron oxide@lignin nanospheres was achieved, which improved the stability and dispersibility of magnetic nanoparticles and enabled them to form beautiful structural colors under the action of an external magnetic field, in line with the concept of sustainable chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895565A_ABST
    Figure CN118895565A_ABST
Patent Text Reader

Abstract

The invention discloses a ferroferric oxide-lignin nanosphere with a core-shell structure as well as a preparation method and application of the ferroferric oxide-lignin nanosphere. The method comprises the following steps: uniformly mixing a lignin solution and a monodisperse ferroferric oxide nanoparticle solution, volatilizing an organic solvent by stirring to obtain a monodisperse ferroferric oxide and lignin nanosphere suspension, and carrying out magnet separation to obtain the ferroferric oxide and lignin nanosphere with the core-shell structure. The method is simple, tedious modification treatment on lignin is not needed, conditions are mild, the solvent can be recovered through condensation and liquefaction, the sustainable chemical concept is met, and large-scale preparation of the ferroferric oxide-lignin nanospheres is easy to achieve; the prepared ferroferric oxide and lignin nanospheres have excellent dispersity and uniformity, the stability of magnetic nanoparticles is effectively improved, the magnetic nanoparticles can show beautiful structural color under the action of an external magnetic field, and the ferroferric oxide and lignin nanospheres have great application prospects in the advanced optical field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomass composite materials, and specifically relates to core-shell structured ferroferric oxide@lignin nanospheres and a preparation method and application thereof. Background Art

[0002] Lignin is a natural polymer that is widely present in plants and has a wide range of applications in biomedicine, energy, cosmetics, and construction. Among them, lignin nanospheres have good size controllability, antioxidant properties, water dispersibility, and stability, and show good potential value in natural polymer-based structural color materials. At present, lignin-based photonic crystals usually first need to modify or multiple grade lignin to prepare nanospheres of uniform size, and then use external forces such as centrifugal force as a driving force to complete the construction. However, in order to control the color of photonic crystals, it is necessary to synthesize a series of nanospheres of different sizes, which poses certain obstacles to their practical application.

[0003] Iron tetroxide (Fe tetroxide) colloidal photonic crystals with highly negative surface charge have been shown to be able to adjust the distance between particles by simply adjusting the magnetic field size to obtain photonic crystals of different colors due to their non-dense stacking structure and high dispersibility. However, Fe tetroxide has problems of poor chemical stability and poor colloidal stability during use or long-term storage, and inevitably requires some synthetic polymers or inorganic materials as a protective shell, which is contrary to the current trend of sustainability and health requirements. The preparation of core-shell structured nanospheres with Fe tetroxide as the core and co-assembly with lignin not only improves the stability of Fe tetroxide, but also enables the controllable construction of lignin-based photonic crystals. However, the existing preparation methods of Fe tetroxide@lignin nanospheres or other inorganic materials@lignin nanospheres still have technical difficulties such as difficulty in controlling the number of cores, poor coating effect, and the need for cumbersome chemical modification of lignin. Therefore, it is urgent to develop a simple and green method to achieve the efficient and controllable preparation of monodisperse Fe3O4@lignin nanospheres, which is of great significance for promoting the research of lignin-based structural color materials in the field of advanced optics. Summary of the invention

[0004] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing core-shell structured ferroferric oxide@lignin nanospheres.

[0005] A method for preparing core-shell structured ferroferric oxide@lignin nanospheres with simple core process, mild preparation conditions, and scalable and controllable preparation, wherein ferroferric oxide with high negative charge on the surface is synthesized by a one-pot method, and is used as the assembly core in a volatile organic solvent / water binary solvent, and a simple stirring volatilization method is used to prepare magnetic nanospheres with regular morphology and uniform size. The monodisperse magnetic nanospheres combine the superparamagnetism of ferroferric oxide with the antioxidant and high dispersibility of nano-lignin, and can form photonic crystals with beautiful colors under the action of an external magnetic field.

[0006] Another object of the present invention is to provide core-shell structured ferrosoferric oxide@lignin nanospheres prepared by the above preparation method.

[0007] Another object of the present invention is to provide the application of the core-shell structured ferroferric oxide@lignin nanospheres in colloidal photonic crystals.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A method for preparing core-shell structured ferroferric oxide@lignin nanospheres comprises the following steps:

[0010] (1) uniformly mixing lignin with a binary solvent of an organic solvent / water to obtain a lignin solution;

[0011] (2) The monodispersed Fe3O4 nanoparticle solution and the lignin solution are uniformly mixed, and then the organic solvent is volatilized by stirring to obtain a Fe3O4@lignin nanosphere suspension, and the Fe3O4@lignin nanospheres with core-shell structure are separated by a magnet.

[0012] Preferably, the lignin in step (1) is at least one of alkali lignin, enzymatic lignin, lignin sulfate and organic solvent lignin; more preferably, the lignin is at least one of alkali lignin and enzymatic lignin.

[0013] Preferably, the organic solvent in step (1) is at least one of tetrahydrofuran, ethanol, acetone, methanol and N,N-dimethylformamide; more preferably, the organic solvent is at least one of tetrahydrofuran and ethanol.

[0014] Preferably, the ratio of lignin to water in step (1) is (1-4) mg:1 mL.

[0015] Preferably, the volume ratio of the organic solvent to water in step (1) is 1:1 to 50:1; more preferably, the volume ratio of the organic solvent to water is 4:3.

[0016] Preferably, the uniform mixing method in steps (1) and (2) is ultrasonic dispersion.

[0017] Preferably, the solvent of the monodisperse ferroferric oxide nanoparticle solution in step (2) is water.

[0018] Preferably, the concentration of the monodisperse ferroferric oxide nanoparticle solution in step (2) is 5 to 60 mg / mL; more preferably 10 mg / mL.

[0019] Preferably, in step (2), the mass ratio of ferrosoferric oxide nanoparticles to lignin is 1:(1.5-6).

[0020] Preferably, in step (2), the stirring to volatilize the organic solvent is performed by mechanical stirring, the mechanical stirring speed is 200 to 800 rpm, and the stirring time is 6 to 18 hours. After the stirring is completed, the organic solvent is substantially completely volatilized.

[0021] Preferably, the monodisperse ferroferric oxide nanoparticle solution in step (2) is prepared by the following method:

[0022] After anhydrous ferric chloride, alkaline organic salt, carboxyl or amino-containing polymer with a molecular weight of 6000-20000 g / mol, reducing agent, water and organic solvent are mixed and dissolved, inorganic base is added and dissolved, hydrothermal reaction is carried out, and magnetic nanoparticles are separated by magnet to obtain magnetic nanoparticles, which are washed and dispersed in water.

[0023] More preferably, the alkaline organic salt is at least one of anhydrous sodium acetate, anhydrous sodium citrate and anhydrous sodium succinate; the carboxyl or amino-containing polymer with a molecular weight of 6000 to 20000 g / mol is at least one of poly(4-styrenesulfonic acid-comaleic acid) sodium salt, polyvinyl pyrrolidone and sodium polyacrylate; the reducing agent is at least one of L-ascorbic acid and tauroursodeoxycholic acid; the organic solvent is at least one of ethylene glycol, n-butanol and butanediol; the inorganic base is at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0024] More preferably, the ratio of the anhydrous ferric chloride, the alkaline organic salt, the carboxyl or amino-containing polymer with a molecular weight of 6000 to 20000 g / mol, the reducing agent, water, the organic solvent and the inorganic base is 0.13 to 0.52 g: 0.6 to 2.4 g: 0.2 to 0.8 g: 3 to 6 mg: 10 to 60 μL: 8 to 32 mL: 0.12 to 0.48 g.

[0025] More preferably, the temperature of the hydrothermal reaction is 150-250° C., and the time is 6-18 hours.

[0026] More preferably, the monodisperse ferroferric oxide nanoparticle solution in step (2) is prepared by the following method:

[0027] Anhydrous ferric chloride, anhydrous sodium acetate, poly (4-styrene sulfonic acid-co-maleic acid) sodium salt, L-ascorbic acid, water and ethylene glycol are mixed and dissolved in sequence, sodium hydroxide is added and dissolved, a hydrothermal reaction is performed, and magnetic nanoparticles are separated by a magnet to obtain magnetic nanoparticles, which are then washed and dispersed in water.

[0028] More preferably, the ratio of anhydrous ferric chloride, anhydrous sodium acetate, poly(4-styrenesulfonic acid-co-maleic acid) sodium salt, L-ascorbic acid, water, ethylene glycol and sodium hydroxide is 0.26g:1.2g:0.4g:4.5mg:20μL:16mL:0.24g.

[0029] More preferably, the washing refers to washing with an ethanol / water mixture and ultrapure water for 1 to 5 times respectively.

[0030] More preferably, in the ethanol / water mixture, the volume ratio of ethanol to water is 0.3-1.2:1.

[0031] The core-shell structured ferroferric oxide@lignin nanospheres prepared by the above preparation method.

[0032] The application of the core-shell structured ferroferric oxide@lignin nanospheres prepared by the above preparation method in colloidal photonic crystals.

[0033] The present invention takes monodisperse superparamagnetic nanoparticles as the core, utilizes the self-assembly behavior of lignin in an organic solvent / water binary system, and adopts a simple stirring and volatilization method to make lignin grow with magnetic nanoparticles as the core, avoiding the occurrence of multi-core or agglomeration, and obtains monodisperse ferroferric oxide@lignin nanospheres. Lignin as a shell layer can effectively improve the colloidal and chemical stability of magnetic nanoparticles.

[0034] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0035] (1) The present invention provides a method for preparing ferroferric oxide@lignin nanospheres, which does not require cumbersome modification of lignin, has the advantages of simple process and mild conditions, and can recover the solvent by condensation and liquefaction, conforms to the concept of sustainable chemistry, and is easy to achieve large-scale preparation of ferroferric oxide@lignin nanospheres.

[0036] (2) In the process of lignin coating of ferroferric oxide nanoparticles, the present invention adopts a stirring and volatilizing solvent method, which is different from the traditional preparation method of lignin nanospheres (solvent-antisolvent method). There is no need to introduce an additional antisolvent during the coating reaction, thereby avoiding the occurrence of multi-core or aggregation of magnetic nanoparticles.

[0037] (3) The ferroferric oxide@lignin nanospheres prepared in the present invention have excellent dispersibility and uniformity, and effectively improve the stability of magnetic nanoparticles. They can show beautiful structural colors under the action of an external magnetic field, and have great application prospects in the field of advanced optics. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a scanning electron microscope image of the ferroferric oxide@lignin nanospheres prepared by the method of Example 1.

[0039] Figure 2 This is a transmission electron micrograph of ferroferric oxide@lignin nanospheres prepared by the method of Example 1.

[0040] Figure 3 This is the particle size distribution diagram of the ferroferric oxide@lignin nanospheres prepared by the method of Example 1.

[0041] Figure 4 Magnetic hysteresis loop diagram of ferroferric oxide nanoparticles and ferroferric oxide@lignin nanospheres prepared by the method of Example 1.

[0042] Figure 5 This is a photonic crystal photo of the ferroferric oxide@lignin nanospheres prepared by the method of Example 1 under the action of a magnetic field.

[0043] Figure 6 This is a scanning electron microscope image of ferroferric oxide@lignin nanospheres prepared by the method of Example 2.

[0044] Figure 7 This is a scanning electron microscope image of ferroferric oxide@lignin nanospheres prepared by the method of Example 3.

[0045] Figure 8 The particle size diagram of ferroferric oxide nanoparticles and ferroferric oxide@lignin nanospheres prepared by the methods of Examples 4-6.

[0046] Fig. 9 This is a scanning electron microscope image of ferroferric oxide@lignin nanospheres prepared by the method of Comparative Example 1.

[0047] Fig.10 This is a scanning electron microscope image of ferroferric oxide@lignin nanospheres prepared by the method of Comparative Example 2. DETAILED DESCRIPTION

[0048] The present invention is further described in detail below in conjunction with examples and drawings, but the embodiments of the present invention are not limited thereto.

[0049] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.

[0050] Example 1

[0051] A method for preparing core-shell structured ferroferric oxide@lignin nanospheres comprises the following steps:

[0052] (1) 0.26 g of anhydrous ferric chloride, 1.2 g of anhydrous sodium acetate, 0.4 g of poly(4-styrenesulfonic acid-comaleic acid) sodium salt (purchased from Aladdin, item number P107093), 4.5 mg of L-ascorbic acid and 20 μL of ultrapure water were added to 16 mL of ethylene glycol in sequence and stirred with a magnetic stirrer (600 rpm) until completely dissolved. Then 0.24 g of sodium hydroxide was added and stirred continuously at the same stirring speed until completely dissolved. The obtained solution was transferred to a 25 mL hydrothermal reactor and reacted at 190 ° C for 9 h. After cooling to room temperature, the obtained magnetic nanoparticles were separated by a magnet and washed three times with 15 mL of ethanol / ultrapure water mixed solvent (volume ratio 1:1) and 15 mL of ultrapure water, respectively, to obtain 125 mg of ferroferric oxide nanoparticles, which were finally dispersed in 12.5 mL of ultrapure water.

[0053] (2) 90 mg of alkali lignin was placed in a 100 mL beaker, 70 mL of tetrahydrofuran / ultrapure water binary solvent (volume ratio 4:3) was added, and ultrasonic treatment was performed for 5 min until the alkali lignin was completely dissolved to obtain a lignin solution.

[0054] (3) 2 mL of the ferroferric oxide nanoparticle dispersion obtained in step (1) was added to the lignin solution obtained in step (2), and ultrasonic treatment was performed for 5 min to completely disperse it. Then, stirring was continued for 6 h on a mechanical stirrer at 400 rpm. After the tetrahydrofuran in the mixed solution was completely volatilized, the ferroferric oxide@lignin nanospheres were obtained by magnetic separation.

[0055] Figure 1 This is a scanning electron microscope image of the ferroferric oxide@lignin nanospheres prepared in Example 1 of the present invention. Figure 2 This is a transmission electron microscope image of the ferroferric oxide@lignin nanospheres prepared in Example 1 of the present invention. Figure 3 This is a particle size distribution diagram of the ferroferric oxide@lignin nanospheres prepared in Example 1 of the present invention. Figure 4 Magnetic hysteresis loop diagram of ferroferric oxide nanoparticles and ferroferric oxide@lignin nanospheres prepared by the method of Example 1 of the present invention. Figure 5 This is a photonic crystal of ferroferric oxide@lignin nanospheres prepared by the method of Example 1 of the present invention under the action of a magnetic field. Figure 1 and Figure 2It can be seen that the ferroferric oxide@lignin nanospheres prepared by the method of the present invention have uniform size and regular morphology, and the ferroferric oxide nanoparticles are uniformly coated with lignin. As shown in Figure 3, the average size of the ferroferric oxide@lignin nanospheres prepared in Example 1 of the present invention is 183.7 nm, and the polydispersity coefficient is only 0.059. Figure 4 It can be seen that the ferroferric oxide@lignin nanospheres prepared in the present invention still maintain superparamagnetism after being coated with lignin. Under the action of ordinary strong magnetic magnets, the ferroferric oxide@lignin nanospheres prepared in the present invention can be assembled into a structural color material with beautiful colors, and the strength of the magnetic force can be controlled by changing the distance between the magnet and the sample, thereby obtaining Figure 5 .

[0056] Example 2

[0057] A method for preparing core-shell structured ferroferric oxide@lignin nanospheres is substantially the same as the method in Example 1, except that the lignin raw material in Example 2 is enzymatically hydrolyzed lignin.

[0058] Figure 6 This is a scanning electron microscope image of the ferroferric oxide @ lignin nanospheres prepared in Inventive Example 2. After testing, the ferroferric oxide @ lignin nanospheres prepared in Example 2 have uniform size and regular morphology, and the ferroferric oxide nanoparticles are uniformly coated with lignin, with no significant change compared to Example 1.

[0059] Example 3

[0060] A method for preparing core-shell structured ferroferric oxide@lignin nanospheres is substantially the same as the method in Example 1, except that the organic solvent in Example 3 is ethanol.

[0061] Figure 7 This is a scanning electron microscope image of the ferroferric oxide @ lignin nanospheres prepared in Inventive Example 3. After testing, the ferroferric oxide @ lignin nanospheres prepared in Example 3 have uniform size and regular morphology, and the ferroferric oxide nanoparticles are uniformly coated with lignin, with no significant change compared to Example 1.

[0062] Embodiment 4-6

[0063] A method for preparing core-shell structured ferroferric oxide @ lignin nanospheres is basically the same as the preparation method in Example 1, except that: by adjusting the amount of lignin used in the preparation process (30, 60, 120 mg), core-shell structured ferroferric oxide @ lignin nanospheres of different sizes are prepared.

[0064] Figure 8The particle size diagram of ferroferric oxide nanoparticles and ferroferric oxide@lignin nanospheres prepared by the methods of invention examples 4-6. After testing, the sizes of ferroferric oxide@lignin nanospheres prepared in examples 4-6 are larger than ferroferric oxide nanoparticles, and their sizes increase with the increase of initial lignin concentration.

[0065] Comparative Example 1

[0066] A method for preparing ferroferric oxide@lignin nanospheres comprises the following steps:

[0067] (1) 0.26 g of anhydrous ferric chloride, 1.2 g of anhydrous sodium acetate, 0.4 g of poly(4-styrenesulfonic acid-comaleic acid) sodium salt (purchased from Aladdin, item number P107093), 4.5 mg of L-ascorbic acid and 20 μL of ultrapure water were added to 16 mL of ethylene glycol in sequence and stirred with a magnetic stirrer (600 rpm) until completely dissolved. Then 0.24 g of sodium hydroxide was added and stirred continuously at the same stirring speed until completely dissolved. The obtained solution was transferred to a 25 mL hydrothermal reactor and reacted at 190 ° C for 9 h. After cooling to room temperature, the obtained magnetic nanoparticles were separated by a magnet, washed three times with 15 mL of ethanol / ultrapure water mixed solvent (volume ratio 1:1) and 15 mL of ultrapure water, respectively, and finally dispersed in 12.5 mL of ultrapure water.

[0068] (2) 90 mg of alkali lignin was placed in a 100 mL beaker, added to 40 mL of tetrahydrofuran solution, and ultrasonically treated for 5 min until the alkali lignin was completely dissolved to obtain a lignin solution.

[0069] (3) Add 2 mL of the ferroferric oxide nanoparticle dispersion obtained in step (1) to the lignin solution obtained in step (2), perform ultrasonic treatment for 5 min to completely disperse it, then add 60 mL of ultrapure water at a rate of 4 mL / min, and continue stirring at 400 rpm on a mechanical stirrer for 6 h. After the tetrahydrofuran in the mixed solution is completely volatilized, separate it with a magnet to obtain ferroferric oxide@lignin nanospheres.

[0070] Fig. 9 This is a scanning electron microscope image of the ferroferric oxide@lignin nanospheres prepared by the method of Comparative Example 1. Fig. 9 It can be seen that compared with Example 1, the coating effect of the ferroferric oxide @ lignin nanospheres prepared by adding an antisolvent to the solvent for self-assembly is not good, and multi-core and aggregation occur, which shows that monodisperse core-shell structured ferroferric oxide @ lignin nanospheres cannot be prepared under the condition of introducing the antisolvent later. The reason is that with the addition of the antisolvent, local lignin molecules will be induced to spontaneously nucleate preferentially, and combine with nearby ferroferric oxide nanoparticles during the assembly process to form multi-core nanospheres.

[0071] Comparative Example 2

[0072] A method for preparing ferroferric oxide@lignin nanoparticles comprises the following steps:

[0073] (1) 0.26 g of anhydrous ferric chloride, 1.2 g of anhydrous sodium acetate, 0.4 g of poly(4-styrenesulfonic acid-comaleic acid) sodium salt (purchased from Aladdin, item number P107093), 4.5 mg of L-ascorbic acid and 20 μL of ultrapure water were added to 16 mL of ethylene glycol in sequence and stirred with a magnetic stirrer (600 rpm) until completely dissolved. Then 0.24 g of sodium hydroxide was added and stirred continuously at the same stirring speed until completely dissolved. The obtained solution was transferred to a 25 mL hydrothermal reactor and reacted at 190 ° C for 9 h. After cooling to room temperature, the obtained magnetic nanoparticles were separated by a magnet, washed three times with 15 mL of ethanol / ultrapure water mixed solvent (volume ratio 1:1) and 15 mL of ultrapure water, respectively, and finally dispersed in 12.5 mL of ultrapure water.

[0074] (2) 90 mg of alkali lignin was placed in a 100 mL beaker, 70 mL of tetrahydrofuran / ultrapure water binary solvent (volume ratio 4:3) was added, and ultrasonic treatment was performed for 5 min until the alkali lignin was completely dissolved to obtain a lignin solution.

[0075] (3) 2 mL of the ferroferric oxide nanoparticle dispersion obtained in step (1) was added to the lignin solution obtained in step (2), and the mixture was subjected to ultrasonic treatment for 5 min to completely disperse the mixture, and then placed under an exhaust fan for 36 h. After the tetrahydrofuran in the mixture was completely volatilized, the ferroferric oxide@lignin nanoparticles were separated by a magnet.

[0076] Fig.10 This is a scanning electron microscope image of the ferroferric oxide@lignin nanospheres prepared by the method of comparative example 2. Fig.10 It can be seen that compared with Example 1, the ferroferric oxide @ lignin nanoparticles prepared without stirring during the solvent evaporation process showed cross-linking and aggregation, which means that monodispersed core-shell structured ferroferric oxide @ lignin nanospheres cannot be prepared even if the continuous stirring process of the lignin solution and the ferroferric oxide nanoparticles is omitted. The reason is that the lack of stirring treatment makes it impossible for the magnetic nanoparticles to maintain good dispersion during the assembly process, resulting in cross-linking and aggregation between the lignin shells.

[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing core-shell structured ferroferric oxide@lignin nanospheres, characterized in that: The steps include: (1) uniformly mixing lignin with a binary solvent of an organic solvent / water to obtain a lignin solution; (2) The monodispersed Fe3O4 nanoparticle solution and the lignin solution are uniformly mixed, and then the organic solvent is volatilized by stirring to obtain a Fe3O4@lignin nanosphere suspension, and the Fe3O4@lignin nanospheres with core-shell structure are separated by a magnet.

2. The method for preparing a core-shell structured ferroferric oxide@lignin nanosphere according to claim 1, characterized in that: The organic solvent in step (1) is at least one of tetrahydrofuran, ethanol, acetone, methanol and N,N-dimethylformamide; the volume ratio of the organic solvent to water in step (1) is 1:1 to 50:

1.

3. The method for preparing a core-shell structured ferroferric oxide@lignin nanosphere according to claim 1, characterized in that: In step (2), the mass ratio of ferroferric oxide nanoparticles to lignin is 1:(1.5-6); The lignin in step (1) is at least one of alkali lignin, enzymatic lignin, lignin sulfate and organic solvent lignin.

4. The method for preparing a core-shell structured ferroferric oxide@lignin nanosphere according to claim 1, characterized in that: The ratio of lignin to water in step (1) is (1-4) mg:1 mL; The concentration of the monodisperse ferroferric oxide nanoparticle solution in step (2) is 5 to 60 mg / mL.

5. The method for preparing a core-shell structured ferroferric oxide@lignin nanosphere according to claim 1, characterized in that: In step (2), the volatile organic solvent is stirred by mechanical stirring, and the mechanical stirring speed is 200 to 800 rpm; the stirring time is 6 to 18 hours.

6. The method for preparing a core-shell structured ferroferric oxide@lignin nanosphere according to claim 1, characterized in that: In step (1), the lignin is at least one of alkali lignin and enzymatic lignin; and the organic solvent is at least one of tetrahydrofuran and ethanol.

7. The method for preparing a core-shell structured ferroferric oxide@lignin nanosphere according to claim 1, characterized in that: The monodisperse ferroferric oxide nanoparticle solution in step (2) is prepared by the following method: anhydrous ferric chloride, alkaline organic salt, a carboxyl or amino-containing polymer with a molecular weight of 6000 to 20000 g / mol, a reducing agent, water and an organic solvent are mixed and dissolved in sequence, an inorganic base is added and dissolved, a hydrothermal reaction is carried out, and magnetic nanoparticles are separated by a magnet, which are then washed and dispersed in water.

8. The method for preparing core-shell structured ferroferric oxide@lignin nanospheres according to claim 7, characterized in that: The alkaline organic salt is at least one of anhydrous sodium acetate, anhydrous sodium citrate and anhydrous sodium succinate; the carboxyl or amino-containing polymer with a molecular weight of 6000 to 20000 g / mol is at least one of poly(4-styrenesulfonic acid-comaleic acid) sodium salt, polyvinyl pyrrolidone and sodium polyacrylate; the reducing agent is at least one of L-ascorbic acid and tauroursodeoxycholic acid; the organic solvent is at least one of ethylene glycol, n-butanol and butanediol; the inorganic base is at least one of sodium hydroxide, potassium hydroxide and lithium hydroxide; The ratio of anhydrous ferric chloride, alkaline organic salt, carboxyl or amino-containing polymer with a molecular weight of 6000 to 20000 g / mol, reducing agent, water, organic solvent and inorganic base is 0.13 to 0.52 g: 0.6 to 2.4 g: 0.2 to 0.8 g: 3 to 6 mg: 10 to 60 μL: 8 to 32 mL: 0.12 to 0.48 g; The temperature of the hydrothermal reaction is 150-250° C. and the time is 6-18 hours.

9. A core-shell structured ferroferric oxide@lignin nanosphere prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the core-shell structured ferroferric oxide@lignin nanospheres as described in claim 9 in colloidal photonic crystals.

Citation Information

Patent Citations

  • Monodisperse superparamagnetic nano crystal colloidal core-shell composite particles and preparation method thereof

    CN103342393A

  • Shell-core magnetic lignin-modified phenolic microsphere adsorbent and preparation method thereof

    CN107469796A

  • Preparation method of polymer magnetic bead used for protein separation

    CN108636305A

  • Lignin-compounded magnetic thermoplastic elastomer and preparation method thereof

    CN110467761A

  • Preparation method and application of magnetic lignin adsorption material

    CN115845812A