Acid boiling destressing device and acid boiling annealing destressing method
Through the acid boiling stress removal device and the acid boiling annealing method, the stress removal problem in the preparation of YAG laser rods is solved, which significantly improves the beam quality and performance of the laser, and achieves a higher extinction ratio and laser performance improvement.
Patent Information
- Application Number
- CN202411003121.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, the stress generated by the YAG laser rod during the preparation process is difficult to completely remove, affecting the beam quality of the laser, especially in the field of high precision, which has an adverse impact on laser performance.
The acid boiling stress removal device and the acid boiling annealing method are used to remove mechanical stress by reacting with the crystal rod by acidic medium, and combined with the support structure and annealing treatment, the extinction ratio and laser performance are improved.
Effectively reduce the mechanical stress in the crystal rod, improve the beam quality of the laser, significantly improve the extinction ratio and other performance indicators, and improve laser performance.
Smart Images

Figure CN118895566A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of crystal rod preparation, and in particular to an acid boiling stress relief device and an acid boiling annealing stress relief method. Background Art
[0002] YAG laser rods, i.e. yttrium aluminum garnet crystal rods doped with rare earth ions, are the core working material of a widely used solid-state laser, the "YAG laser". They can be divided into: Nd:YAG crystal, Nd:Ce:YAG crystal, Yb:YAG crystal, etc. The laser rods used in laser marking machines and other industrial laser equipment are generally Nd:YAG crystals.
[0003] During the normal growth and preparation of YAG laser rods, stress will be generated inside, which will have an adverse effect on the quality of the laser beam when the crystal rods are assembled into lasers. In the prior art, the measure to eliminate stress is to simply perform conventional annealing. Although the stress can be partially eliminated, some residual stress will still remain. In the field of high-precision laser applications, the adverse effect of this residual stress on laser performance cannot be ignored.
[0004] The extinction ratio is an important quantitative indicator for measuring the performance of laser crystals. It reflects the light transmission characteristics of the crystal under different polarization states, characterizes the magnitude of the depolarization loss caused by stress birefringence formed by certain defects in the laser crystal, and is an important parameter for determining laser performance such as Q switching and frequency doubling. Its definition is to place the laser crystal between parallel polarizers and orthogonal polarizers, use a light source to be incident from one end of the crystal, measure the optical power at the output end, and obtain two values P∥ and P⊥ respectively. The extinction ratio is the ratio of P∥ and P⊥, take its logarithm and multiply it by 10, and the unit is dB. The larger the extinction ratio value, the smaller the stress inside the crystal. Summary of the invention
[0005] The purpose of the present invention is to provide an acid boiling stress relief device and an acid boiling annealing method for obtaining a high-quality crystal rod preparation method to address the above-mentioned deficiencies, thereby solving the problem in the prior art that there is no simple and efficient device for removing stress from the crystal rod.
[0006] The present invention is achieved through the following scheme:
[0007] A stress relief device for acid boiling includes at least but not limited to a heating component, a first containing tank and a second containing tank; the second containing tank is arranged in the first containing tank, and the first containing tank is provided with a support frame for lifting the second containing tank; a heating medium is arranged in the first containing tank, an acid medium is arranged in the second containing tank, and a support structure for restricting a crystal rod is also arranged in the second containing tank.
[0008] Based on the structure of the above-mentioned acid boiling stress relief device, the heating component specifically adopts an electric heating furnace, and the bottom of the first containing tank is in direct contact with the electric heating furnace.
[0009] Based on the structure of the above-mentioned acid boiling stress relief device, the support frame includes support legs and a support plate, the support plate is a hollow structure as a whole, the support plate includes a support ring and a support rod, the support rod is arranged on the support ring at intervals, and the support legs are obliquely arranged on the support ring.
[0010] Based on the structure of the above-mentioned acid boiling stress relief device, the first containing tank is a truncated cone structure with one end open, the large circular surface of the first containing tank is open, and the small circular surface is in contact with the heating component.
[0011] Based on the structure of the above-mentioned acid boiling stress relief device, the second containing tank is a straight cylindrical structure.
[0012] Based on the structure of the above-mentioned acid boiling stress relief device, a hollow glass cover is provided on the second containing tank. The hollow glass cover is a liquid level truncated cone structure as a whole. The hollow glass cover is covered on the straight cylindrical second containing tank.
[0013] Based on the structure of the above-mentioned acid boiling stress relief device, a counterweight block is arranged in the second containing tank, and the material of the counterweight block is the same as that of the crystal rod to be acid boiled.
[0014] Based on the structure of the above-mentioned acid boiling stress relief device, the support structure includes a support plate, and a plurality of V-shaped grooves are arranged on the end surface of the support plate away from the ground of the second containing tank. The V-shaped grooves are arranged at intervals, and the size of the V-shaped grooves is adapted to the structure of the crystal rod to be acid boiled.
[0015] Based on the structure of the above-mentioned acid boiling stress relief device, the material of the support plate is the same as that of the crystal rod to be acid boiled.
[0016] The present invention also provides an acid boiling annealing stress relief method, which comprises at least the following steps:
[0017] Step 1: Rough selection of raw materials, preliminary screening from crystal blanks: Use a stress meter to perform stress inspection on the blanks and preliminarily screen out high-quality blanks;
[0018] Step 2: Raw material cutting: Cut the selected blank material according to its appearance and the internal quality of the crystal;
[0019] Step 3: The raw materials are initially shaped and ground. The cut square bars are initially ground to process the rough cut surfaces and grind out the vertical surfaces. According to the design requirements, the round bars are ground to the specified diameter or the square bars are ground to the specified width and thickness.
[0020] Step 4: Laser marking and coding: Use a laser marking machine to engrave the product serial number on the cylindrical surface of the round bar or the side of the square bar for coding;
[0021] Step 5: Acid boiling treatment: put the engraved square or round bar into the acid boiling treatment device, and preset the time, temperature and other parameters; the purpose of this step is to eliminate the mechanical stress caused by the previous processing and improve the extinction ratio;
[0022] Step 6: Annealing: After cleaning and wiping the acid-boiled square bars or round bars, put them into the annealing furnace, preset the corresponding parameters, and perform high-temperature annealing treatment (1200-1300℃, constant temperature time 20-200 hours) to further improve and stabilize the performance index of the extinction ratio and improve other properties of the square bars;
[0023] Step 7: Detection: Detect the extinction ratio and transmission wavefront distortion of the square or round bar after acid boiling and annealing, and record and save the detection data;
[0024] Step 8: Polish, roughly grind, finely polish the beveled end surface and coat the square bars or round bars, and finally inspect and put them into storage.
[0025] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0026] 1. This solution heats the acidic medium by means of constant temperature heating to avoid violent boiling of the acidic medium caused by local high temperature. The acidic medium can be heated gently and the stress of the crystal rod in the second holding tank can be removed. The principle of stress removal is that the mechanical stress in the crystal rod is removed by the reaction between the acidic medium and the crystal rod. At the same time, a support structure is set in the second holding tank to isolate each crystal rod to avoid collision between crystal rods during the acid boiling stress removal process, thereby avoiding damage to the crystal rod.
[0027] 2. This solution can reduce the mechanical stress in the crystal rod, thereby improving the quality of the crystal rod. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the overall structure of the present invention;
[0029] Figure 2 It is a schematic diagram of the top view of the support frame in the present invention;
[0030] Figure 3 This is the stress instrument detection image of 35.5*7.5*149.5 large square strip after acid boiling;
[0031] Figure 4 This is the image of a 35.5*7.5*149.5 square bar after acid boiling and annealing.
[0032] Figure 5 This is a stress instrument comparison chart of normal annealing after acid boiling and normal annealing without acid boiling;
[0033] Description of the drawings: 1. Heating component; 2. First containing tank; 3. Second containing tank; 4. Support frame; 5. Heating medium; 6. Acidic medium; 7. Hollow glass cover; 8. Counterweight block; 9. Support plate; 10. V-shaped groove; 11. Crystal rod; 41. Support leg; 42. Support ring; 43. Support rod. DETAILED DESCRIPTION
[0034] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0035] Any feature disclosed in this specification (including any additional claims and abstract), unless otherwise stated, may be replaced by other equivalent or alternative features having similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0036] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0037] In addition, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features.
[0038] Example 1
[0039] like Figure 1-2 As shown, the present invention provides a technical solution:
[0040] An acid boiling stress relief device, which at least includes but is not limited to a heating component 1, a first containing tank 2 and a second containing tank 3; the second containing tank 3 is arranged in the first containing tank 2, and the first containing tank 2 is provided with a support frame 4 for lifting the second containing tank 3; a heating medium 5 is arranged in the first containing tank 2, an acidic medium 6 is arranged in the second containing tank 3, and the second containing tank 3 is also provided with a support structure for limiting crystal rods.
[0041] Based on the above structure, the present solution heats the acidic medium 6 by means of constant temperature heating to avoid violent boiling of the acidic medium 6 caused by local high temperature. The acidic medium 6 can be heated gently and stress removal can be performed on the crystal rods in the second holding tank 3. The principle of stress removal is that the mechanical stress in the crystal rods is removed by reacting the acidic medium 6 with the crystal rods. At the same time, a support structure is provided in the second holding tank 3 to isolate each crystal rod to avoid collision between the crystal rods during the acid boiling stress removal process, thereby preventing damage to the crystal rods.
[0042] As an example, the heating component 1 may be an electric heating furnace, and the bottom of the first containing tank 2 is in direct contact with the electric heating furnace.
[0043] Based on the above structure, the first holding tank 2 is directly heated by an electric heating furnace to heat the heating medium 5, and the heating medium 5 transfers the temperature to the second holding tank 3, so that the part of the second holding tank 3 immersed in the heating medium 5 can be evenly heated.
[0044] As an example, the support frame 4 may include support legs 41 and a support plate. The support plate is a hollow structure as a whole. The support plate includes a support ring 42 and a support rod 43. The support rod 43 is arranged on the support ring 42 at intervals, and the support legs 41 are obliquely arranged on the support ring 42.
[0045] Based on the above structure, the support plate is set as a hollow structure, so that the bottom of the second containing tank 3 can also be in contact with the heating medium 5 as much as possible, so that the heating of the second containing tank 3 is more even.
[0046] As an example, the first containing groove 2 is a truncated cone structure with one end open. The large circular surface of the first containing groove 2 is open, and the small circular surface is in contact with the heating component 1.
[0047] As an example, the second containing tank 3 is a straight cylindrical structure, and a hollow glass cover 7 can be provided on the second containing tank 3 . The hollow glass cover 7 is a liquid level truncated cone structure as a whole, and the hollow glass cover 7 covers the straight cylindrical second containing tank 3 .
[0048] Based on the above structure, the hollow glass cover 7 is provided to facilitate covering the second containing tank 3 on the one hand, reduce the heat loss of the acidic medium 6 during heating, and maintain a constant temperature; on the other hand, the acidic medium 6 can be condensed on the top of the glass cover and then reflux into the second containing tank 3, reducing the evaporation loss of the acidic medium 6.
[0049] As an example, a counterweight block 8 may be provided in the second containing tank 3. The material of the counterweight block 8 is the same as that of the crystal rod to be pickled. This can avoid introducing impurities therein and affecting the pickled crystal rod.
[0050] As an example, the support structure may include a support plate 9, on the end surface of the support plate 9 away from the ground of the second containing tank 3, a plurality of V-grooves 10 may be provided, the V-grooves 10 are arranged at intervals, and the size of the V-grooves 10 is adapted to the structure of the crystal rod to be pickled.
[0051] Based on the above structure, when the crystal rod is placed on the support plate 9, the sharp ends between adjacent V-grooves 10 can automatically space the crystal rods, and the spaced crystal rods can roll into the V-grooves 10, so that each V-groove 10 can be fixed to prevent the crystal rods from colliding with each other due to the boiling acidic medium 6 inside after heating.
[0052] As an example, the material of the support plate 9 is the same as the material of the crystal rod to be pickled.
[0053] As an example, the acidic medium 6 may be concentrated hydrochloric acid, and the heating medium 5 may be water;
[0054] As an example, the second containing tank may be made of glass.
[0055] Example 2
[0056] like Figures 3 to 5 As shown, based on the structure of the above-mentioned embodiment 1, the present invention provides a technical solution:
[0057] An acid boiling annealing stress relief method comprises at least the following steps:
[0058] Step 1: Rough selection of raw materials, preliminary screening from blanks: Use a stress meter to check the stress of the blanks and preliminarily screen out high-quality blanks;
[0059] Step 2: Raw material cutting: Cut the selected blank material according to its appearance and the internal quality of the crystal;
[0060] Step 3: The raw materials are initially shaped and ground. The cut square bars are initially ground to process the rough cut surfaces and grind out the vertical surfaces. According to the design requirements, the round bars are ground to the specified diameter or the square bars are ground to the specified width and thickness.
[0061] Step 4: Laser marking and coding: Use a marking machine to engrave the product serial number on the cylindrical surface of the round bar or the side of the square bar for coding;
[0062] Step 5: Acid boiling treatment: put the engraved square or round bar into the acid boiling treatment device, and preset the time, temperature and other parameters; the purpose of this step is to eliminate the mechanical stress caused by the previous processing and improve the extinction ratio;
[0063] Step 6: Annealing: After cleaning and wiping the acid-boiled square bars or round bars, put them into the annealing furnace, preset the corresponding parameters, and perform high-temperature annealing treatment (1200-1300℃, constant temperature time 20-200 hours) to further improve and stabilize the performance index of the extinction ratio and improve other properties of the square bars;
[0064] Step 7: Detection: Detect the extinction ratio and transmission wavefront distortion of the square or round bar after acid boiling and annealing, and record and save the detection data;
[0065] Step 8: Polish, roughly grind, finely polish the bevel end surface, coat and conduct final inspection on the square bar or round rod.
[0066] In step 5, the specific steps of acid boiling treatment are:
[0067] Add water to the first holding tank, add concentrated hydrochloric acid to the second holding tank, and place a crystal rod on the support plate of the second holding tank. The sharp ends between adjacent V-grooves can automatically space the crystal rods. The spaced crystal rods can roll into the V-grooves so that each V-groove can be fixed. Close the hollow glass cover, turn on the heating component, and heat for 2 to 3 hours.
[0068] In step eight, the polishing process specifically includes polishing the large surface of the square strip and performing protective chamfering. After completion, the large surface shape and smoothness are inspected by quality inspection.
[0069] In step eight, the rough grinding and fine polishing of the beveled end surface specifically include: rough grinding (controlling the size and angle) and fine polishing (surface trimming, etc.) the beveled end surface of the large-surfaced slat;
[0070] In step eight, the coating is specifically as follows: the finished strips are appropriately protected and then sent to the coating workshop for coating;
[0071] In step eight, the final inspection is specifically as follows: the quality inspection department conducts a final inspection on the coated strips and then generates a report, which is marked and protected in the finished product warehouse.
[0072] The following is the specific process of the acid boiling process experiment in this scheme to verify the effect of the acid boiling annealing treatment:
[0073] Experiment 1
[0074] Experimental object: 6 Ф6*98 induction furnace round bars. The stress meter inspection found abnormal stress, which may be structural stress.
[0075] Acid boiling treatment time: 15:04 to 16:34, lasting 1 hour and 30 minutes. About 15 minutes after the temperature started to rise, the acid solution began to boil violently, and the water bath temperature was measured to be constant at 98°C.
[0076] Experimental results: There was no significant improvement in the stress meter inspection. The extinction ratios of two rods, XGR69803 and XGR59801, were randomly tested and were 26.3dB and 27.1dB before treatment and 26.8dB and 27.3dB after treatment.
[0077] Summary: Acid boiling treatment has no obvious effect on the stress caused by defects in the crystal itself.
[0078] Experiment 2
[0079] Experimental objects: 6 round rods from Experiment 1.
[0080] Experimental purpose: To extend the processing time and verify whether the extinction ratio is improved.
[0081] Acid boiling treatment time: 14:03 start - 17:04 end, the process is 3 hours and 1 minute. About 14 minutes after the temperature started to rise, the acid began to boil violently. About 40 minutes later, the boiling phenomenon of the acid weakened to a stable state. The water bath temperature was measured to be constant at 92°C.
[0082] Experimental results: There is no obvious improvement after prolonging the acid boiling time for the Ф6*98 round bar.
[0083] Summary: Prolonging the acid boiling time has no significant effect on improving the stress caused by the crystal's own defects.
[0084] Experiment 3
[0085] Experimental object: 49 4.5*4.5*30 right-angle square bars, checked by stress meter before treatment - stress mainly exists at corners and sides.
[0086] Changes in experimental conditions: It was discussed that repeated use of acid would reduce the acid concentration and may affect the treatment effect, so new concentrated HCL was used this time.
[0087] Acid boiling treatment: starts at 13:55 and ends at 17:00, the whole process takes 3 hours and 5 minutes.
[0088] Annealing treatment: 49 4.5*4.5*30 right-angle square bars are placed in 6# annealing furnace for annealing treatment, and the parameters are set to 1300℃, 100H for annealing.
[0089] Experimental results: 7 out of 49 4.5*4.5*30 were unqualified due to other reasons after rough polishing, 11 were returned as excess materials, and the remaining 31 were finely polished, and the extinction ratio test results were better than expected, and the stress was eliminated to a great extent. The extinction ratio test results are shown in the following table:
[0090]
[0091] Experiment 4
[0092] Experimental object: 1 7.5*35.5*149.5 slat.
[0093] Experimental purpose: Previously, some small-sized square bars or round bars were subjected to acid boiling annealing to relieve stress, which showed good results. However, for products with longer lengths or larger diameters, the improvement effect needs to be verified. The purpose of this experiment is mainly to verify the stress relief effect of acid boiling annealing on large square bars.
[0094] Experimental process: from 14:00 to 17:00, duration 3 hours.
[0095] Experimental results: 35.5*7.5*149.5 After preliminary observation by the stress meter, the two wide surfaces showed different stress distributions. The stress on one side had been removed, while the stress on the other side remained. Figure 3 As shown in the experiment, the gray side shows that the stress has not been eliminated, and the extinction ratio is low, with a value of about 18dB to 19dB. After recording the information, the large strip was put into the annealing furnace on January 29. After annealing, the stress was observed by the stress meter and the stress was good. Figure 4 .
[0096] After the acid annealing treatment, the extinction ratio was tested and compared with the extinction ratio of the previous test without acid annealing treatment. The data are as follows:
[0097]
[0098] By comparison, it can be seen that after the large square strips were acid boiled and normally annealed, their extinction ratio was greatly improved.
[0099] Experiment 5
[0100] Experimental purpose: Taking 20 pieces of 5.5*5.5*L blanks (cut out from the same single crystal) from the induction furnace as the object, we divided them into two batches, 10 pieces in each batch, and tested the extinction ratios of the initial state, after simple acid boiling, after simple normal annealing, and acid boiling plus normal annealing. The extinction ratio data were used to summarize and evaluate the effects of simple acid boiling, simple normal annealing, and acid boiling followed by normal annealing on stress removal.
[0101] We numbered all the induction furnace samples, tested their extinction ratios and recorded them as the initial data A of the experiment, as shown in Table 1:
[0102] Table 1 Initial data of extinction ratio measured for 20 samples A
[0103]
[0104]
[0105] Data B, we divided the 20 samples into two parts according to the number, each part has 10 pieces, and the 10 samples numbered 11-20 were acid-boiled. The extinction ratio of the 10 samples after acid boiling was tested. The data is shown in Table 2:
[0106] Table 2 Extinction ratio data of 10 samples (No. 11-20) B
[0107]
[0108] The "improvement value" is the improvement and enhancement of the extinction ratio of the same sample after acid boiling relative to the initial data A.
[0109] Data C, we annealed all 20 samples normally according to the previous annealing process, and then tested the extinction ratio, and obtained data C as shown in Table 3:
[0110] Table 3 Extinction ratio data of 20 samples (No. 1-20) C
[0111]
[0112] The "improvement values" numbered 11-20 are the values of the extinction ratio of the same sample after acid boiling annealing compared with data B; the "improvement values" numbered 1-10 are the values of the extinction ratio of the same sample after only annealing compared with data A. The stress distribution is observed by the stress meter, such as Figure 5 shown.
[0113] The left side is a sample that was annealed after acid boiling, and the right side is a sample that was annealed directly without acid boiling. It can be observed from the figure that the sample that was not acid boiled showed two light yellow areas at the edges, which means that some stress has not been removed; while the sample on the left side that was acid boiled and annealed is almost the same as the background color (purple red) transmitted in the field of view of the stress meter, and no other color blocks are shown, indicating that the stress has been basically removed.
[0114] Compared with the initial data A, the total improvement value of the extinction ratio is shown in Table 4:
[0115] Table 4 Overall extinction ratio improvement after the experiment
[0116]
[0117]
[0118] Through these three sets of data, we can compare and analyze the effects of the three treatment processes of pure acid boiling, pure annealing and acid boiling plus annealing on sample stress and draw conclusions.
[0119] Comparing the data A and data B of samples No. 11-20, we can see the extent to which simple acid boiling can remove stress from the samples: the extinction ratio improvement value is basically above 10dB. Conclusion: Acid boiling treatment can improve the extinction ratio to a certain extent (stress removal is effective).
[0120] Comparing data B and data C of samples No. 11-20, we can get the influence of acid boiling plus annealing and simple acid boiling on the stress of the same sample: the extinction ratio after acid boiling plus annealing is improved compared with simple acid boiling, with the improvement ranging from 3.8 to 13.8 dB. Conclusion: Acid boiling annealing is better than simple acid boiling in terms of stress removal effect.
[0121] Comparing data C and data B of samples No. 1-10, although they are not the same samples, can roughly reflect which of the two treatment processes, simple acid boiling and simple annealing, has a better effect on stress removal. Conclusion: Simple annealing is better than simple acid boiling in terms of stress removal effect.
[0122] Analyzing and comparing data C, we can roughly reflect which of the two treatment processes, simple annealing and acid boiling annealing, is better at removing stress. Conclusion: In terms of stress removal effect, acid boiling annealing is better than simple annealing.
[0123] Based on the above comparison and analysis, it can be concluded that acid boiling annealing is the best way to remove stress.
[0124] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An acid boiling stress relief device, characterized in that: At least including but not limited to a heating component, a first holding tank and a second holding tank; the second holding tank is arranged in the first holding tank, and the first holding tank is provided with a support frame for lifting the second holding tank; the first holding tank is provided with a heating medium, the second holding tank is provided with an acidic medium, and the second holding tank is also provided with a support structure for restricting the crystal rod.
2. The acid boiling stress relief device according to claim 1, characterized in that: The heating component specifically adopts an electric heating furnace, and the bottom of the first containing tank is in direct contact with the electric heating furnace.
3. The acid boiling stress relief device according to claim 2, characterized in that: The support frame includes support legs and a support plate. The support plate is a hollow structure as a whole. The support plate includes a support ring and a support rod. The support rod is arranged on the support ring at intervals. The support legs are obliquely arranged on the support ring.
4. The acid boiling stress relief device according to claim 3, characterized in that: The first containing groove is a truncated cone structure with one end open. The large circular surface of the first containing groove is open, and the small circular surface is in contact with the heating component.
5. The acid boiling stress relief device according to claim 4, characterized in that: The second containing tank is a straight cylindrical structure.
6. The acid boiling stress relief device according to claim 5, characterized in that: The second containing tank is provided with a hollow glass cover, the hollow glass cover is a liquid level truncated cone structure as a whole, and the hollow glass cover is covered on the straight cylindrical second containing tank.
7. The acid boiling stress relief device according to claim 6, characterized in that: A counterweight block is arranged in the second containing tank, and the material of the counterweight block is the same as that of the crystal rod to be acid-boiled.
8. The acid boiling stress relief device according to claim 7, characterized in that: The support structure comprises a support plate, on the end surface of the support plate away from the ground of the second containing tank is provided with a plurality of V-shaped grooves, the V-shaped grooves are arranged at intervals, and the size of the V-shaped grooves is adapted to the structure of the crystal rod to be acid-boiled.
9. The acid boiling stress relief device according to claim 8, characterized in that: The material of the support plate is the same as that of the crystal rod to be acid-boiled.
10. A method for relieving stress by acid boiling annealing, characterized in that: At least the following steps are included: Step 1: Rough selection of raw materials, preliminary screening from crystal blanks: Use a stress meter to perform stress inspection on the blanks and preliminarily screen out high-quality blanks; Step 2: Raw material cutting: Cut the selected blank material according to its appearance and the internal quality of the crystal; Step 3: Initial shaping and grinding of raw materials. Initial grinding of the cut square bars, processing of the rough surface of the cut and grinding of the vertical surface; grinding of round bars to the specified diameter or grinding of square bars to the specified width and thickness according to design requirements; Step 4: Laser marking and coding: Use a laser marking machine to engrave the product serial number on the cylindrical surface of the round bar or the side of the square bar for coding; Step 5: Acid boiling treatment: put the engraved square or round bar into the acid boiling treatment device and preset the time and temperature parameters; the purpose of this step is to eliminate the mechanical stress caused by the previous processing and improve the extinction ratio; Step 6: Annealing: After cleaning and wiping the acid-boiled square bar or round bar, put it into the annealing furnace, preset the corresponding parameters, and perform high-temperature annealing treatment to further improve and stabilize the measured value of the extinction ratio and improve the performance of the square bar or round bar; Step 7: Detection: Detect the extinction ratio and transmission wavefront distortion of the square or round bar after acid boiling and annealing, and record and save the detection data; Step 8: Polish, roughly grind, finely polish the beveled end surface and coat the square bars or round bars, and then conduct final inspection and put them into storage.