Cool-feeling split-type composite fiber as well as preparation method and application of cool-feeling split-type composite fiber

The cooling lobe-type composite fiber combined with polygonal star core layer and petal fan-shaped cortex solves the problem of short-term effect of cool fabrics in the prior art, realizes the continuous cooling and efficient heat conduction of the fibers, and is suitable for textiles, improving the Comfortable to wear.

CN118895579AInactive Publication Date: 2024-11-05TAI CHI STONE (SHANGHAI) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075713.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118895579A_ABST
    Figure CN118895579A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional fibers, and particularly relates to a cool-feeling split type composite fiber and a preparation method and application thereof. In the cool-feeling splinter-type composite fiber provided by the invention, polyamide has good moisture absorption and sweat releasing performance and strong conduction and heat dissipation capability, and is partially exposed, so that sweat or moisture can be rapidly conducted and evaporated, and the cool feeling of a fabric is strong; the moisture regain of the polyamide is higher than that of other fibers, the moisture content of the polyamide is high in the same environment, and the cool feeling of the polyamide is stronger; according to the present invention, the polyester has characteristics of excellent heat conduction and heat dissipation performance and rapid heat conduction, and the cool feeling functional master batch has characteristics of slow heat absorption and rapid heat dissipation, and has a high thermal diffusion coefficient, and the thermal diffusion coefficient can achieve 10 <-4 > m < 2 > / s, such that the splinter type composite fiber has characteristics of continuous cooling, moisture conduction, rapid drying, slow temperature rising and long-acting cooling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional fibers, and in particular relates to a cool-feeling split-type composite fiber and a preparation method and application thereof. Background Art

[0002] Cool fiber is a kind of fiber that can prevent discomfort when wet and has excellent cold touch feeling. Its principle is to utilize the medium (cool factor) in nature that absorbs heat slowly and dissipates heat quickly, add it to carriers such as polyester, nylon or regenerated cellulose fiber, and prepare the resulting cool functional masterbatch into cool fiber. When the skin touches the woven fabric, it will produce excellent cool feeling.

[0003] At present, the development of cool fabrics can be divided into two categories in principle: one is to improve the thermal conductivity of textiles and enhance the ability of textiles to dissipate heat to the environment; the other is to improve the hygroscopicity and water conductivity of textiles so that human sweat can be quickly absorbed and discharged by clothing, and the purpose of heat dissipation can be achieved through sweat evaporation. There are three main technologies for the development of cool fabrics: one is to use fibers that have a cool feeling, or to prepare fibers that can achieve a cool feeling through physical or chemical modification, and then use the fibers to prepare cool fabrics; the second is to achieve the cool effect of fabrics through the design of fabric organization and structure; the third is to give fabrics a cool feeling through fabric finishing.

[0004] However, most fabrics only achieve an instantaneous, short-term cool-to-touch effect. Summary of the invention

[0005] The object of the present invention is to provide a cooling lobe-type composite fiber and a preparation method and application thereof. The cooling lobe-type composite fiber provided by the present invention has excellent instant cooling sensation, and the cooling sensation is maintained for a long time.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a cooling lobe-type composite fiber, comprising a core layer and a skin layer wrapped on the outer surface of the core layer; the cross-sectional shape of the core layer is a polygonal star shape; the cross-sectional shape of the skin layer is a petal fan shape; the cross-sectional shape of the cooling lobe-type composite fiber is a circle formed by the core layer and the skin layer; the corner surface of the polygonal star shape is not wrapped with the skin layer; the core layer comprises polyamide; the skin layer comprises polyester and cooling functional masterbatch.

[0008] Preferably, the number of corners in the polygonal star shape is 4 to 8.

[0009] Preferably, the discontinuity width of the cortex is 0.015 to 0.040 mm.

[0010] Preferably, the mass ratio of the core layer to the skin layer is 30-50:50-70.

[0011] Preferably, the diameter of the cooling split-type composite fiber is 1.0 to 1.4 mm.

[0012] The present invention also provides a method for preparing the cool split-type composite fiber described in the above scheme, comprising the following steps:

[0013] Pre-crystallizing, drying and first melt extruding the polyamide in sequence to obtain a core layer component;

[0014] The cooling function masterbatch and the polyester are mixed and then melt-extruded for the second time to obtain a skin layer component;

[0015] The core layer component and the skin layer component are extruded and formed, and then shaped to obtain a cool split-type composite fiber.

[0016] Preferably, the pre-crystallization temperature is 40-150° C. and the time is within 20 minutes.

[0017] Preferably, the drying temperature is 30-100°C, the pressure is 60-120 kPa, the drying atmosphere is air, and the air flow rate is 100-180 m 3 / h until the moisture content of the dried material is less than 300ppm.

[0018] Preferably, the temperature of the first melt extrusion is 250-280° C., and the screw speed is 15-70 rpm; the temperature of the second melt extrusion is 270-300° C., and the screw speed is 15-70 rpm.

[0019] The present invention also provides the use of the cool-feeling split-type composite fiber described in the above scheme or the cool-feeling split-type composite fiber obtained by the preparation method described in the above scheme in textiles.

[0020] The present invention provides a cool-feeling split-type composite fiber. In the cool-feeling split-type composite fiber provided by the present invention, polyamide has good moisture absorption and perspiration performance, and the thermal conductivity is 0.244-0.337W / (m·℃), while polyester is 0.084W / (m·℃), and cotton is 0.071-0.073W / (m·℃). It has a high thermal conductivity and strong conduction and heat dissipation capacity, and is partially exposed, so that sweat or water can be quickly conducted and evaporated, and the fabric has a strong cool feeling; and the moisture regain of polyamide (4.5%) is higher than that of other fibers, and its moisture content will also be high under the same environment, and its cool feeling will also be stronger; polyester has excellent thermal conductivity and heat dissipation performance, and can quickly conduct heat. The cool-feeling functional masterbatch has the characteristics of slow heat absorption and fast heat dissipation, and has a high thermal diffusion coefficient, and the thermal diffusion coefficient reaches 10 -4 m 2 / s (The thermal diffusion coefficient of ordinary rocks is about 10-6 m 2 / s, the thermal diffusion coefficient of the cooling functional masterbatch is two orders of magnitude higher than that of ordinary rocks), thus giving the split-type composite fiber of the present invention the characteristics of continuous cooling, moisture conduction and quick drying, slow temperature rise and long-lasting cooling. The results of the embodiment show that the instantaneous cooling coefficient Qmax value of the fabric prepared by the fabric reaches 0.30, the continuous cooling feeling reaches level 1, the evaporation rate reaches 0.35, the antibacterial rate against Staphylococcus aureus is greater than 99%, the antibacterial rate against Klebsiella pneumoniae is greater than 96%, the antibacterial rate against Candida albicans is greater than 93%, and the anti-ultraviolet performance UPF value is 50+.

[0021] The present invention also provides a method for preparing the cooling split-type composite fiber described in the above scheme. The cooling split-type composite fiber provided by the present invention not only has excellent instant cooling feeling, but also maintains the cooling feeling for a long time, and the fabric prepared by the cooling split-type composite fiber has the same cooling effect as the wearing time increases.

[0022] The present invention also provides the use of the cool-splitting composite fiber described in the above scheme or the cool-splitting composite fiber obtained by the preparation method described in the above scheme in textiles. The cool-splitting composite fiber provided by the present invention utilizes the synergistic effect of the excellent thermal conductivity of polyester and the excellent moisture absorption and perspiration performance of polyamide to accelerate the rapid evaporation of water in the fiber, thereby achieving a better cooling effect, having an excellent effect of combining coolness and dryness, being suitable for use in textiles, and greatly improving the comfort of wearing. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 The lobe cross section of the cool lobe type composite fiber provided by the present invention;

[0025] Figure 2 The present invention provides a cross section of a cool-feeling split-type composite fiber after alkali treatment. DETAILED DESCRIPTION

[0026] The present invention provides a cooling lobe-type composite fiber, comprising a core layer and a skin layer wrapped on the outer surface of the core layer; the cross-sectional shape of the core layer is a polygonal star shape; the cross-sectional shape of the skin layer is a petal fan shape; the cross-sectional shape of the cooling lobe-type composite fiber is a circle formed by the core layer and the skin layer; the corner surface of the polygonal star shape is not wrapped with the skin layer; the core layer comprises polyamide; the skin layer comprises polyester and cooling functional masterbatch.

[0027] The cool split-type composite fiber provided by the present invention comprises a core layer; the number of corners in the multi-pointed star shape is preferably 4 to 8, more preferably 5 to 7, and further preferably 6 (such as Figure 1 The corners are preferably evenly distributed on the circumference of the core layer cross section; the cross-sectional shape of the core layer is preferably a "M" shape or a "X" shape.

[0028] In the present invention, the core layer comprises polyamide, and the polyamide is preferably hygroscopic polyamide; the moisture absorption rate of the hygroscopic polyamide is preferably 5.5-6.8%, more preferably 5.8-6.4%, and further preferably 6.0%.

[0029] The cool-feeling split-type composite fiber provided by the present invention includes a cortex wrapped on the outer surface of the core layer; the intermittent width of the cortex (the width of the corners of the polygonal star not wrapped by the cortex) is preferably 0.015-0.040 mm, more preferably 0.020-0.035 mm, and further preferably 0.025-0.030 mm.

[0030] In the present invention, the cooling functional masterbatch is preferably the cooling functional masterbatch described in CN113527850A.

[0031] In the present invention, the mass ratio of the core layer to the skin layer is preferably 30-50:50-70, more preferably 35-45:55-65, and further preferably 40-42:60-62.

[0032] In the present invention, the cross-sectional shape of the cooling split-type composite fiber is circular. The present invention adopts a circular shape, which has the smallest specific surface area and is the most stable.

[0033] In the present invention, the diameter of the cooling split-type composite fiber is preferably 1.0 to 1.4 mm, more preferably 1.1 to 1.3 mm, and further preferably 1.2 mm.

[0034] The present invention also provides a method for preparing the cool split-type composite fiber described in the above scheme, comprising the following steps:

[0035] Pre-crystallizing, drying and first melt extruding the polyamide in sequence to obtain a core layer component;

[0036] The cooling function masterbatch and the polyester are mixed and then melt-extruded for the second time to obtain a skin layer component;

[0037] The core layer component and the skin layer component are extruded and formed, and then shaped to obtain a cool split-type composite fiber.

[0038] The present invention sequentially pre-crystallizes, dries and first melt-extrudes the polyamide to obtain a core layer component. In the present invention, the viscosity of the polyamide is preferably 1.600-1.610 dl / g, more preferably 1.603-1.607 dl / g, and further preferably 1.605 dl / g.

[0039] In the present invention, the pre-crystallization temperature is preferably 40-150° C., more preferably 60-120° C., and further preferably 80-100° C.; the pre-crystallization time is preferably within 20 min, and more preferably 5-15 min.

[0040] In the present invention, the drying temperature is preferably 30 to 100°C, more preferably 50 to 80°C, the pressure is preferably 60 to 120 kPa, more preferably 80 to 100 kPa, the drying atmosphere is preferably air, and the air flow rate is preferably 100 to 180 m 3 / h, more preferably 130 to 150m 3 / h until the moisture content of the dried material is less than 300ppm.

[0041] In the present invention, the pre-crystallization and drying equipment is preferably a crystallization dryer.

[0042] In the present invention, the first melt extrusion equipment preferably includes a screw extruder, a filter, a spinning manifold and a split-type composite assembly connected in sequence; the temperature of the first melt extrusion is preferably 250-280°C, more preferably 260-270°C, and the screw speed is preferably 15-70rpm, more preferably 30-50rpm; the screw extruder preferably includes zones 1 to 5 and a flange zone; the temperature of zone 1 is preferably 255-260°C, more preferably 256-259°C, and further preferably 257-258°C; the temperature of zone 2 is preferably 266-272°C, It is more preferably 268-271°C, and further preferably 269°C; the temperature of the third zone is preferably 266-272°C, more preferably 267-270°C, and further preferably 270°C; the temperature of the fourth zone is preferably 266-272°C, more preferably 268-271°C, and further preferably 269°C; the temperature of the fifth zone is preferably 266-272°C, more preferably 267-270°C, and further preferably 268°C; the temperature of the flange zone is preferably 259-265°C, more preferably 260-264°C, and further preferably 261-263°C.

[0043] The present invention mixes the cooling function masterbatch and the polyester and then performs a second melt extrusion to obtain the skin layer component. In the present invention, the viscosity of the polyester is preferably 0.670 to 0.680 dl / g, more preferably 0.673 to 0.677 dl / g, and further preferably 0.675 dl / g.

[0044] In the present invention, the second melt extrusion equipment preferably includes a screw extruder, a spinning manifold and a split-type composite assembly connected in sequence; the temperature of the second melt extrusion is preferably 270-300°C, more preferably 280-290°C, and the screw speed is preferably 15-70rpm, more preferably 30-50rpm; the screw extruder preferably includes zones 1 to 5 and a flange zone; the temperature of zone 1 is preferably 255-260°C, more preferably 256-259°C, and further preferably 257-258°C; the temperature of zone 2 is preferably 270-275°C, more preferably 270-275°C The temperature of the third zone is preferably 278-280°C, more preferably 278-279°C, and further preferably 279°C; the temperature of the fourth zone is preferably 276-278°C, more preferably 276-277°C, and further preferably 277°C; the temperature of the fifth zone is preferably 274-276°C, more preferably 274-275°C, and further preferably 275°C; the temperature of the flange zone is preferably 258-260°C, more preferably 258-259°C, and further preferably 259°C.

[0045] After obtaining the core layer component and the skin layer component, the present invention extrudes and shapes the core layer component and the skin layer component to obtain a cool-feeling split-type composite fiber. In the present invention, the extrusion molding equipment preferably includes a split-type composite spinning assembly; the cross-sectional shape of the split-type composite spinning assembly is the same as the cross-sectional shape of the cool-feeling split-type composite fiber.

[0046] In the present invention, the extrusion molding is preferably carried out under the condition of monomer suction; the equipment for monomer suction is preferably a monomer suction device; the circulating motor pressure of the monomer suction device is preferably 0.5-1.0MPa, more preferably 0.7-0.8MPa, and the spinning position suction pressure is preferably 0.3-0.8MPa, more preferably 0.5-0.6MPa.

[0047] In the present invention, the setting preferably includes cooling setting and stretching setting performed in sequence; the cooling setting is preferably air cooling; the air cooling is preferably side blowing air cooling; the air cooling temperature is preferably 20-22°C, more preferably 21°C, the humidity is preferably 65-75%, more preferably 70%, and the wind speed is preferably 0.30-0.60m / s, more preferably 0.40-0.50m / s; the stretching temperature of the stretching setting is preferably 70-110°C, more preferably 80-90°C, the setting temperature is preferably 80-150°C, more preferably 100-120°C, and the stretching ratio is preferably 1.0-3.0, more preferably 2.0.

[0048] In the present invention, the stretching and shaping process preferably further comprises oiling the product obtained by cooling and shaping.

[0049] In the present invention, after the stretching and shaping, the product obtained by the stretching and shaping is preferably wound; the winding speed is preferably 2500-5000 m / min, more preferably 3500-4500 m / min.

[0050] The cool split-type composite fiber prepared by the invention has a linear density of 50-200D, a breaking strength of 3.5-4.8 cN / dtex, and a breaking elongation of 25-50%.

[0051] The present invention also provides the use of the cool-feeling split-type composite fiber described in the above scheme or the cool-feeling split-type composite fiber obtained by the preparation method described in the above scheme in textiles.

[0052] The cool split composite fiber provided by the present invention is suitable for textiles, especially for cool textiles, such as knitted stretch double-sided fabrics, and the fabric is subjected to conventional alkali treatment to open the fibers (such as Figure 2 As shown in the figure, the different shrinkage of the skin-core components in alkali solution will weaken the strength of the combined section of the two and cause the skin-core layers to peel apart, which will give the fabric a good capillary wicking effect, excellent moisture conduction and dyeability, and good wearing comfort.

[0053] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0054] Example 1

[0055] In this embodiment, the hygroscopic polyamide slice (moisture absorption rate is 6.0%) is produced by Fujian Yongrong Jinjiang Co., Ltd. and has a viscosity of 1.605 dl / g; the hygroscopic polyamide slice is pre-crystallized and dried in a crystallization dryer at a crystallization temperature of 80°C, a drying temperature of 50°C, a drying air pressure of 100 kPa, and a flow rate of 180 m 3 / h to obtain dried hygroscopic polyamide chips with a moisture content of <150ppm; then melt-extruded through the first screw extruder to obtain a polyamide melt, which is transported to the spinning manifold and evenly distributed into the split-type composite assembly to obtain a core layer component; wherein the temperatures of zones 1 to 5 and the flange zone of the first screw extruder are 255°C, 266°C, 266°C, 266°C, 266°C and 259°C, respectively, and the screw speed is 18rpm.

[0056] In this embodiment, the cool functional masterbatch is the commercially available CN113527850A cool jade masterbatch, and the polyester chips are produced by Jiangsu Hengli Chemical Fiber Co., Ltd. and have a viscosity of 0.677dl / g; the cool functional masterbatch and the polyester chips are mixed, melt-extruded through a second screw extruder to obtain a cool polyester melt, which is then transported to a spinning box and evenly distributed into a split-type composite assembly to obtain a cortex component; wherein the temperatures of zones 1 to 5 and the flange zone of the second screw extruder are 260°C, 275°C, 280°C, 278°C, 276°C and 260°C, respectively, and the screw speed is 50rpm.

[0057] The core layer component and the skin layer component are uniformly extruded and formed through a split-type composite spinning assembly, the monomer is sucked, the side-blown air is cooled and formed, oiled, stretched and shaped, and wound. The mass ratio of the core layer to the skin layer is 3:7, the spinning box temperature is 280°C, the circulating motor pressure of the monomer suction device is 0.60MPa, the suction pressure at the spinning position is 0.70MPa, the side-blowing (without wind tube frame) wind speed is 0.35m / s, the cooling temperature is 21.0°C, the humidity is 67.5%, the stretching temperature is 75°C, the shaping temperature is 135°C, the stretching ratio is 3.2 times, and the winding speed is 3600m / min to obtain a cool split-type composite fiber with a single fiber fineness of 2.29dtex, a breaking strength of 3.83cN / dtex, an elongation at break of 32.90%, and a complete skin-core cross-section without shedding.

[0058] Example 2

[0059] In this embodiment, the hygroscopic polyamide slice (moisture absorption rate is 6.0%) is produced by Fujian Yongrong Jinjiang Co., Ltd. and has a viscosity of 1.605 dl / g; the hygroscopic polyamide slice is pre-crystallized and dried in a crystallization dryer at a crystallization temperature of 80°C, a drying temperature of 50°C, a drying air pressure of 100 kPa, and a flow rate of 180 m 3 / h to obtain dried hygroscopic polyamide chips with a moisture content of <150ppm; then melt-extruded through the first screw extruder to obtain a polyamide melt, which is transported to the spinning manifold and evenly distributed into the split-type composite assembly to obtain a core layer component; wherein the temperatures of zones 1 to 5 and the flange zone of the first screw extruder are 258°C, 269°C, 269°C, 269°C, 269°C and 262°C, respectively, and the screw speed is 19rpm.

[0060] In this embodiment, the cool functional masterbatch is the commercially available CN113527850A cool jade masterbatch, and the polyester chips are produced by Jiangsu Hengli Chemical Fiber Co., Ltd. with a viscosity of 0.677dl / g. The cool functional masterbatch and the polyester chips are mixed, melt-extruded through a second screw extruder to obtain a cool polyester melt, which is then transported to the spinning box and evenly distributed into the split-type composite assembly to obtain a cortex component; wherein the temperatures of zones 1 to 5 and the flange zone of the second screw extruder are 258°C, 273°C, 278°C, 276°C, 274°C and 258°C, respectively, and the screw speed is 48rpm.

[0061] The core layer component and the skin layer component are uniformly extruded and formed through a split-type composite spinning assembly, the monomer is sucked, the side-blown air is cooled and formed, oiled, stretched and shaped, and wound. The mass ratio of the core layer to the skin layer is 3.5:6.5, the spinning box temperature is 283°C, the circulating motor pressure of the monomer suction device is 0.62MPa, the suction pressure at the spinning position is 0.73MPa, the side-blowing (without wind tube frame) wind speed is 0.38m / s, the cooling temperature is 21.0°C, the humidity is 67.5%, the stretching temperature is 75°C, the shaping temperature is 135°C, the stretching ratio is 3.4 times, and the winding speed is 3700m / min to obtain a cool split-type composite fiber with a single fiber fineness of 2.75dtex, a breaking strength of 3.96cN / dtex, an elongation at break of 33.25%, and a complete skin-core cross-section without shedding.

[0062] Example 3

[0063] In this embodiment, the hygroscopic polyamide slice (moisture absorption rate is 6.0%) is produced by Fujian Yongrong Jinjiang Co., Ltd. and has a viscosity of 1.605 dl / g. The hygroscopic polyamide slice is pre-crystallized and dried in a crystallization dryer at a crystallization temperature of 80°C, a drying temperature of 50°C, a drying air pressure of 100 kPa, and a flow rate of 180 m 3 / h to obtain dried hygroscopic polyamide chips with a moisture content of <150ppm, which are then melt-extruded through the first screw extruder to obtain a polyamide melt, which is transported to the spinning manifold and evenly distributed into the split-type composite assembly to obtain a core layer component; wherein the temperatures of zones 1 to 5 and the flange zone of the first screw extruder are 260°C, 272°C, 272°C, 272°C, 272°C and 265°C, respectively, and the screw speed is 20rpm.

[0064] In this embodiment, the cool functional masterbatch is the commercially available CN113527850A cool jade masterbatch, and the polyester chips are produced by Jiangsu Hengli Chemical Fiber Co., Ltd. with a viscosity of 0.677dl / g. The cool functional masterbatch and the polyester chips are mixed, melt-extruded through a second screw extruder to obtain a cool polyester melt, which is then transported to the spinning box and evenly distributed into the split-type composite assembly to obtain a cortex component; wherein the temperatures of zones 1 to 5 and the flange zone of the second screw extruder are 255°C, 270°C, 280°C, 278°C, 276°C and 260°C, respectively, and the screw speed is 47rpm.

[0065] The core layer component and the skin layer component are uniformly extruded and formed through a split-type composite spinning assembly, the monomer is sucked, the side-blown air is cooled and formed, oiled, stretched and shaped, and wound. The mass ratio of the core layer to the skin layer is 4:6, the spinning box temperature is 285°C, the circulating motor pressure of the monomer suction device is 0.65MPa, the suction pressure at the spinning position is 0.76MPa, the side-blowing (without wind tube frame) wind speed is 0.40m / s, the cooling temperature is 21.0°C, the humidity is 67.5%, the stretching temperature is 75°C, the shaping temperature is 140°C, the stretching ratio is 3.1 times, and the winding speed is 3800m / min to obtain a cool split-type composite fiber with a single fiber fineness of 3.21dtex, a breaking strength of 4.08cN / dtex, an elongation at break of 33.20%, and a complete skin-core cross-section without shedding.

[0066] Test Case

[0067] The cool lobe-type composite fiber prepared in Examples 1 to 3 was woven into a fabric (knitted stretch double-sided fabric), the content of the cool lobe-type composite fiber in the fabric was 30wt%, the prepared fabric had an instantaneous cool coefficient Qmax value of 0.3, a contact coolness of level 1, an evaporation rate of 0.35, an inhibition rate against Staphylococcus aureus of >99%, an inhibition rate against Klebsiella pneumoniae of >96%, an inhibition rate against Candida albicans of >93%, and an anti-ultraviolet performance UPF value of 50+.

[0068] It can be seen from the above embodiments that the cooling split-type composite fiber provided by the present invention has excellent instant cooling effect, and the cooling effect is maintained for a long time. The cooling effect of the fabric prepared by the cooling split-type composite fiber remains unchanged as the wearing time increases.

[0069] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A cool-feeling split-type composite fiber, It is characterized in that It comprises a core layer and a skin layer wrapped around the outer surface of the core layer; The cross-sectional shape of the core layer is a polygonal star; the cross-sectional shape of the cortex layer is a petal fan; The cross-sectional shape of the cooling split-type composite fiber is a circle formed by the core layer and the skin layer; The corner surfaces of the polygonal star are not covered with cortex; The core layer comprises polyamide; the skin layer comprises polyester and cool-feeling functional masterbatch.

2. The cool split-type composite fiber according to claim 1, It is characterized in that The number of corners in the polygonal star is 4 to 8.

3. The cool split-type composite fiber according to claim 1, It is characterized in that The intermittent width of the cortex is 0.015 to 0.040 mm.

4. The cool split-type composite fiber according to claim 1 or 3, It is characterized in that The mass ratio of the core layer to the skin layer is 30-50:50-70.

5. The cool split-type composite fiber according to claim 1 or 2, It is characterized in that The diameter of the cooling split-type composite fiber is 1.0 to 1.4 mm.

6. A method for preparing the cool split-type composite fiber according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Pre-crystallizing, drying and first melt extruding the polyamide in sequence to obtain a core layer component; The cooling function masterbatch and the polyester are mixed and then melt-extruded for the second time to obtain a skin layer component; The core layer component and the skin layer component are extruded and formed, and then shaped to obtain a cool split-type composite fiber.

7. The preparation method according to claim 6, It is characterized in that The temperature of the pre-crystallization is 40-150° C. and the time is within 20 minutes.

8. The preparation method according to claim 6, It is characterized in that The drying temperature is 30-100°C, the pressure is 60-120 kPa, the drying atmosphere is air, and the air flow rate is 100-180 m 3 / h until the moisture content of the dried material is less than 300ppm.

9. The preparation method according to claim 6 or 7, It is characterized in that The temperature of the first melt extrusion is 250-280° C., and the screw speed is 15-70 rpm; the temperature of the second melt extrusion is 270-300° C., and the screw speed is 15-70 rpm.

10. Use of the cool-feeling split-type composite fiber according to any one of claims 1 to 5 or the cool-feeling split-type composite fiber obtained by the preparation method according to any one of claims 6 to 9 in textiles.