Construction technology of reed foil rattan plaster suspended ceiling
By using wooden keels to fix reed foil in ancient buildings and using a specific three-layer mortar plastering process, the problems of excessive weight and prone to cracking in traditional ceilings are solved, and the overall weight of the ceiling and the strength of the ash layer are reduced, which protects the ancient The cultural value of architecture.
Patent Information
- Application Number
- CN202411074934.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-05
AI Technical Summary
The traditional reed foil smear-painted ash ceiling construction technology leads to excessive weight of the ceiling and reduced load-bearing capacity during the renovation of ancient buildings, which can easily cause ceiling cracks. The difficulty of painting and decoration after modern technology construction increases, affecting the protection of the cultural value of ancient buildings.
Using a construction process similar to the ancient method, the reed foil is fixed with wooden keels and a specific three-layer mortar plastering process, including the combination of ripe lime, hemp knife, bluestone powder, polypropylene staple fiber and nanosilicon dioxide, ensure the ceiling The overall weight is relatively light, and the ash layer is firmly combined with the reed foil to prevent the ash layer from cracking.
It has achieved a reduction in the overall weight of the suspended ceiling, met the special requirements for the repair of ancient buildings, improved the strength and crack resistance of the ash layer, protected traditional construction technology, facilitated painting and decoration, and had important cultural value protection significance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of ancient building construction, and in particular to a construction process for a reed foil and hemp ash ceiling. Background Art
[0002] The suspended ceiling is a decorative layer under the upper floor or roof of the room for sound insulation, noise prevention and heat preservation. It is more important in the entire room decoration and can also decorate the top of the room. Most of the ancient Chinese houses, palaces, pavilions and other buildings are civil structures, and the top space of the interior is basically dominated by wooden structures. The main materials used for the suspended ceiling are bamboo rafts, reed foil, fabrics, etc. The reed foil ceiling, which uses wooden keels to fix lead wires to hang reed foil, is a common ceiling structure in ancient buildings. It has the characteristics of environmental protection, naturalness and comfort. The outer layer of the above-mentioned reed foil ceiling is decorated with gray backing, which is a reed foil smeared hemp knife gray ceiling. This kind of ceiling is flatter and convenient for painting decoration on the gray backing.
[0003] The traditional construction technology of reed foil and hemp plaster ceiling mostly uses wooden hanging, wooden strips and reed foil to hang the ceiling, and then thinly plasters the ceiling. In the construction of ancient residential buildings, the requirements for the flatness and use of the ceiling were relatively low, and the above-mentioned construction technology was more convenient. The existing reed foil and hemp plaster ceiling is mostly used for the repair of ancient buildings, and has higher requirements for the flatness and use of the ceiling.
[0004] The reed foil and hemp ash ceiling currently used in the repair of ancient buildings is limited by the construction requirements and the application of current construction technology, and the construction process has been greatly different from the traditional process. The construction process of the reed foil and hemp ash ceiling currently used in the repair of ancient buildings mostly uses wood-plastic keels and uses lime mortar, mixed mortar and / or cement mortar to plaster the ceiling. Some construction processes will also use new waterproof membranes, such as SBS modified asphalt felt, polyurethane waterproofing, EPDM sheet waterproofing, etc. These modern materials and processes can effectively reduce the overall weight of the ceiling to meet the special requirements of the repair of ancient buildings. However, using modern construction technology, although the appearance of the ancient building can be maintained as much as possible after the repair, the difficulty of painting and decorating the ceiling is greatly increased due to problems such as material replacement. However, when repairing ancient buildings using the traditional reed foil and hemp ash ceiling construction technology, the overall weight of the ceiling is relatively large. After a long period of history, the overall bearing capacity of the overall civil structure of the ancient building has been greatly reduced. The construction of the traditional reed foil and hemp ash ceiling will make the building difficult to bear and easily cause problems such as cracking of the ceiling. Summary of the invention
[0005] In order to solve at least one of the above technical problems, a construction method is developed that is easy to operate, can effectively repair the suspended ceiling of ancient buildings, and has a construction process that is closer to the traditional reed foil and hemp ash ceiling construction process. The present application provides a reed foil and hemp ash ceiling construction process.
[0006] The present application provides a construction process for a reed foil and hemp ash ceiling, comprising the following steps: S1. Installation of wooden keels: The main keel wooden beams are arranged along the purlin direction, and the secondary keel wooden beams are arranged at intervals. The keel and the roof beam are fixed with wooden beams as hangers. The lower part of the left and right side beams is nailed to the side of the keel, and the upper part is nailed to the side of the purlin or beam. S2. Installation of hanging nails and reed foil: Fix the finished reed foil to the bottom of the wooden keel with nails. Use more reed foil during installation to ensure that the gap between reed foils is less than 5mm. Then, according to the arrangement of the wooden keel, use nails to wrap thin iron wire for tensioning and maintenance. S3, preparing mortar: preparing the first layer of mortar, the components of which include slaked lime, hemp knife, bluestone powder and nano-silicon dioxide; preparing the second layer of mortar, the components of which include slaked lime, polypropylene staple fiber, nano-silicon dioxide and compatibilizer; preparing the topcoat mortar, the topcoat mortar is prepared according to the weight ratio of slaked lime, hemp knife, polypropylene staple fiber and compatibilizer of 98:1~3:2~4:4~6; S4. Plastering: Use the first coat of plaster to construct a 2~4mm thick inner plaster layer on the outside of the reed foil, use the second coat of plaster to construct a 4~8mm thick middle plaster layer on the outside of the inner plaster layer, and finally use the finishing plaster to construct a 1~3mm thick outer plaster layer on the outside of the middle plaster layer. After the outer plaster layer is constructed, press it repeatedly to make the surface smooth and compact to complete the ceiling construction.
[0007] By adopting the above technical scheme, the present application adopts a construction process similar to the ancient method, using a wooden keel to be fixed to the top of the building in a specific way, and then installing reed foil, and finally using a specific mortar to plaster in a three-layer construction method. On the premise of ensuring that the outer ash layer of the ceiling is close to the traditional ash layer material, the overall weight of the ceiling is relatively light, which can meet the special construction requirements of ancient building repair; the reed foil installation of the present application adopts an encrypted method, and the outer layer of plastering is carried out in a three-layer construction method using mortar with a specific ratio and mixed with hemp. The ash layer is firmly combined with the reed foil, and the ash layer itself has a high strength, which can effectively avoid cracking of the ash layer.
[0008] Optionally, in step S1, the size of the main keel wooden beam is 100mm×60mm, the size of the secondary keel wooden beam is 50mm×50mm, the size of the hanger wooden beam is 70mm×70mm, the secondary keel spacing is 40mm, and the hanger spacing is 1000mm.
[0009] Optionally, in step S2, when the length of the main keel is insufficient, it is overlapped on the side, the overlap length is not less than 50 cm, the overlap is fixed with nails, tied with binding wire, and a suspension rod is added at the overlap.
[0010] Optionally, in step S2, the nails are spaced 30 mm apart.
[0011] Optionally, in step S2, when installing the reed foil, individual reeds are shortened in areas with high density, and areas with large gaps are reinforced with iron wire and a single reed.
[0012] Optionally, in step S3, the weight proportions of the components of the first layer of ash include: 90-100 parts of slaked lime, 4-6 parts of hemp knife, 3-5 parts of bluestone powder, and 6-10 parts of nano-silicon dioxide.
[0013] Optionally, in step S3, the weight proportions of the components of the second layer of ash include: 90-100 parts of slaked lime, 4-6 parts of polypropylene staple fibers, 4-8 parts of nano-silicon dioxide, and 6-8 parts of TPP tricresyl phosphate.
[0014] Optionally, in step S4, the middle ash layer is constructed after the surface of the inner ash layer is 60% to 70% dry, and the middle ash layer needs to be squeezed into the inner ash layer during construction.
[0015] Optionally, in step S4, after the construction of the middle ash layer, the surface needs to be smoothed, and then the texture is processed on the outside.
[0016] Optionally, in step S4, the outer ash layer is constructed after the surface of the middle ash layer is 70% to 80% dry.
[0017] In summary, the present invention includes at least one of the following beneficial technical effects: 1. This application adopts a construction process similar to the ancient method, using wooden keels to be fixed to the top of the building in a specific way, then installing reed foil, and finally using a specific mortar to plaster in a three-layer construction method. On the premise of ensuring that the outer ash layer of the ceiling is close to the material of the traditional ash layer, the overall weight of the ceiling is relatively light, which can meet the special construction requirements of ancient building repair; 2. The reed foil installation of this application adopts an encrypted method. The outer plastering adopts a three-layer construction method using a mortar with a specific ratio and mixed with hemp. The mortar layer is firmly combined with the reed foil, and the mortar layer itself has a high strength, which can effectively prevent the mortar layer from cracking; 3. This application solves the problem of combining traditional ancient building repair technology with modern use, avoids the use of modern technology, which leads to the loss of traditional technology and difficulty in painting and decoration. It is of great significance to the protection of the cultural value of traditional ancient buildings, especially cultural relics and ancient buildings, and has important guiding significance for the use and protection of traditional construction technology in the future. DETAILED DESCRIPTION
[0018] The present application is further described in detail below with reference to the embodiments.
[0019] The present application discloses a construction process for a reed foil-smeared hemp ash ceiling, comprising the following steps: S1. Installation of wooden keels: The main keel wooden beams are arranged along the purlin direction, and the secondary keel wooden beams are arranged at intervals. The keel and the roof beam are fixed with wooden beams as hangers. The lower part of the left and right side beams is nailed to the side of the keel, and the upper part is nailed to the side of the purlin or beam. S2. Installation of hanging nails and reed foil: Fix the finished reed foil to the bottom of the wooden keel with nails. Use more reed foil during installation to ensure that the gap between reed foils is less than 5mm. Then, according to the arrangement of the wooden keel, use nails to wrap thin iron wire for tensioning and maintenance. S3, preparing mortar: preparing the first layer of mortar, the components of which include slaked lime, hemp knife, bluestone powder and nano-silicon dioxide; preparing the second layer of mortar, the components of which include slaked lime, polypropylene staple fiber, nano-silicon dioxide and compatibilizer; preparing the topcoat mortar, the topcoat mortar is prepared according to the weight ratio of slaked lime, hemp knife, polypropylene staple fiber and compatibilizer of 98:1~3:2~4:4~6; S4. Plastering: Use the first coat of plaster to construct a 2~4mm thick inner plaster layer on the outside of the reed foil, use the second coat of plaster to construct a 4~8mm thick middle plaster layer on the outside of the inner plaster layer, and finally use the finishing plaster to construct a 1~3mm thick outer plaster layer on the outside of the middle plaster layer. After the outer plaster layer is constructed, press it repeatedly to make the surface smooth and compact to complete the ceiling construction.
[0020] The following are preparation examples and embodiments of the present application: The main raw materials of the preparation examples and embodiments of this application are all purchased from the market. Among them, nano-silicon dioxide, with a particle size of 100-200 nm, was purchased from Baiyi Mineral Products Processing Plant in Lingshou County; polypropylene staple fiber, model HY-430, was purchased from Shandong Hongyao Copper Materials Co., Ltd.; hemp knives, purchased from Xingtai Juheng Hemp Products Co., Ltd.; TPP tricresyl phosphate, 99% purity, was purchased from Shanghai McLean Biochemical Technology Co., Ltd.
[0021] The following is an example of preparation of this application Preparation Example 1 In this preparation example, quicklime is firstly added with water to be slaked, and then left to stand for no less than 15 days to obtain slaked lime; hemp is beaten into flocculent form with a thin wooden stick.
[0022] The weight proportions of the components of the first coat of ash in this preparation example include: 90 parts of slaked lime, 4 parts of hemp knife, 3 parts of bluestone powder, and 10 parts of nano silicon dioxide.
[0023] When preparing, use a mixer to make mortar, and ensure that the mixer is fully stirred, no less than three times, so that the hemp and ash are mixed evenly. Check the prepared mortar, and make sure that the hemp is not sticky and willowy, and the mortar has no lumps.
[0024] The weight proportions of the components of the second coat of ash in this preparation example include: 90 parts of slaked lime, 4 parts of polypropylene staple fibers, 8 parts of nano-silicon dioxide, and 6 parts of TPP tricresyl phosphate.
[0025] During preparation, first put slaked lime and nano-silicon dioxide in a slurry barrel and use a mixer to make mortar; then put the slurry barrel in an ice water bath, add polypropylene staple fiber and TPP tricresyl phosphate, and use a mixer to fully stir to evenly mix the polypropylene staple fiber and ash.
[0026] The finishing ash of this preparation example is prepared by mixing slaked lime, hemp knife, polypropylene staple fiber and TPP tricresyl phosphate in a weight ratio of 98:1:2:4.
[0027] When preparing, use a mixer to make the mortar. Make sure the mixer is fully stirred for at least three times to make the hemp and ash evenly mixed. Check the prepared mortar to make sure the hemp is not sticky or willowy, and the mortar has no lumps.
[0028] Preparation Example 2 The difference between this preparation example and preparation example 1 lies in the proportion of each mortar.
[0029] The weight proportions of the components of the first coat of ash in this preparation example include: 100 parts of slaked lime, 6 parts of hemp knife, 5 parts of bluestone powder, and 6 parts of nano silicon dioxide.
[0030] The weight proportions of the components of the second coat of ash in this preparation example include: 100 parts of slaked lime, 6 parts of polypropylene staple fibers, 4 parts of nano-silicon dioxide, and 8 parts of TPP tricresyl phosphate.
[0031] The finishing ash of this preparation example is prepared by mixing slaked lime, hemp knife, polypropylene staple fiber and TPP tricresyl phosphate in a weight ratio of 98:3:4:6.
[0032] Preparation Example 3 The difference between this preparation example and preparation example 1 lies in the proportion of each mortar.
[0033] The weight proportions of the components of the first coat of ash in this preparation example include: 94 parts of slaked lime, 5 parts of hemp knife, 4 parts of bluestone powder, and 8 parts of nano silicon dioxide.
[0034] The weight proportions of the components of the second coat of ash in this preparation example include: 96 parts of slaked lime, 5 parts of polypropylene staple fibers, 6 parts of nano-silicon dioxide, and 7 parts of TPP tricresyl phosphate.
[0035] The finishing ash of this preparation example is prepared by mixing slaked lime, hemp knife, polypropylene staple fiber and TPP tricresyl phosphate in a weight ratio of 98:2:3:5.
[0036] The following are examples of the present application:
[0037] Example 1 The construction process of the reed foil smeared hemp ash ceiling of the present embodiment comprises the following steps: S1. Installation of wooden keels: The size of the main keel wood beam is 100mm×60mm, the size of the secondary keel wood beam is 50mm×50mm, and the size of the suspension rod wood beam is 70mm×70mm; the main keel is arranged along the purlin direction, and the secondary keel is set at an interval of 50mm. The keel and the roof beam are fixed with suspension rods, and the spacing between the suspension rods is 1100mm. The lower part of the left and right flashing is nailed to the side of the keel, and the upper part is nailed to the side of the purlin or beam; S2. Installation of nails and reed foil: Fix the finished reed foil to the bottom of the wooden keel with nails first, with the nail spacing of 35mm. The reed foil is used densely during installation to ensure that the gap between the reed foils is less than 5mm. Then, according to the arrangement of the wooden keel, use nails to wrap thin iron wire for tensioning and maintenance. When installing the reed foil, shorten individual reeds in densely populated areas, and reinforce areas with large gaps with iron wire and single reeds. S3, preparing mortar: using the mortar prepared in Preparation Example 1; S4. Plastering: Use the first coat of plaster to construct a 2mm thick inner plaster layer on the outside of the reed foil. Apply a little force with the trowel during construction. While applying force, shake your hands slightly left and right to "knead" the mortar into the seams of the reed foil. Use the second coat of plaster when the inner plaster layer is about 50% dry, then construct a 4mm thick middle plaster layer on the outside. Finally, use the finishing plaster when the middle plaster layer is about 60% dry, then construct a 1mm thick outer plaster layer on the outside. After the outer plaster layer is constructed, press repeatedly to smooth and compact the surface to complete the ceiling construction.
[0038] Example 2 The difference between this embodiment and embodiment 1 is that the mortar of step S2 uses the mortar of preparation example 2.
[0039] Example 3 The difference between this embodiment and embodiment 2 is that the mortar of step S2 uses the mortar of preparation example 3.
[0040] Example 4 The difference between this embodiment and embodiment 3 is that the thickness of the inner ash layer is 4 mm, the thickness of the middle ash layer is 8 mm, and the thickness of the outer ash layer is 3 mm.
[0041] Example 5 The difference between this embodiment and embodiment 3 is that the thickness of the inner ash layer is 3 mm, the thickness of the middle ash layer is 6 mm, and the thickness of the outer ash layer is 2 mm.
[0042] Example 6 The difference between this embodiment and embodiment 5 is that in step S1, the secondary keels are arranged at intervals of 40 mm and the spacing between the suspension rods is 1000 mm.
[0043] Example 7 The difference between this embodiment and embodiment 6 is that in step S1, beams are arranged around the wooden keel, and the beam nails are attached to the sides of the beams or rafters.
[0044] Example 8 The difference between this embodiment and embodiment 7 is that in step S4, the construction of the middle ash layer is carried out after the surface of the inner ash layer is 60% to 70% dry, and the construction of the outer ash layer is carried out after the surface of the middle ash layer is 70% to 80% dry.
[0045] Example 9 The difference between this embodiment and the embodiment 8 is that in step S4, the middle ash layer needs to be squeezed into the inner ash layer during construction.
[0046] Example 10 The difference between this embodiment and embodiment 9 is that in step S4, after the middle ash layer is constructed, the surface is smoothed with a 2m-foot board and swept with a broom to create a pattern.
[0047] Comparative Example 1 The difference between this comparative example and Example 10 is that after the reed foil is installed in step S2, a 5 mm thick polyurethane waterproof layer is coated on the surface of the reed foil, and then a 10 mm thick ash layer is constructed on the outside with cement mortar.
[0048] Comparative Example 2 This comparative example adopts a process that is basically the same as the ancient reed foil and hemp ash ceiling construction process.
[0049] In this comparative example, hemp ash is used on the inner side, and the weight ratio of ash: hemp is 100:5; the middle layer uses mud ash, and the mortar is configured according to the weight ratio of ash: smooth straw at 5:1, and then the mud ash is configured according to the weight ratio of mud: hemp at 100:6; the outer side uses protective mortar, and the weight ratio of ash: hemp is 100:2.
[0050] The difference between this comparative example and Example 10 is that after the reed foil is installed in step S2, the above-mentioned mortar is used for plastering, with the thickness of the inner layer being 35 mm, the thickness of the middle layer being 50 mm, and the thickness of the outer layer being 15 mm.
[0051] The processes of Examples 1 to 8 of the present application were tested for relevant construction quality, mainly testing the weight and overall quality of the suspended ceiling.
[0052] Comparative Example 3 The difference between this comparative example and Example 10 is that in the ratio of the first layer of ash and the second layer of ash, an equal amount of slaked lime is used to replace nano silicon dioxide.
[0053] Comparative Example 4 The difference between this comparative example and Example 10 is that in the ratio of the second coat of ash and the top coat of ash, an equal amount of hemp knife is used to replace the polypropylene staple fiber, and TPP tricresyl phosphate is not added.
[0054] 1. Weight detection According to the size of a 100 square meter building, the ceiling was made using the process of Examples 1 to 10 of the present application, and then the ceiling was made using the process of Comparative Examples 1 to 4. The ceiling of Comparative Example 2 was used as a reference, and the ceiling was weighed to calculate the weight reduction ratio of the ceilings of Examples 1 to 10 of the present application, and the ceilings of Comparative Examples 1, 3, and 4 relative to the ceiling of Comparative Example 2. The results are shown in Table 1.
[0055] Table 1 Weight test results of Examples 1 to 10 and Comparative Examples 1, 3, and 4
[0056] It can be seen from the above test results that the construction technology of the present application is based on the premise that the materials used are very close to those used in the traditional ancient reed foil and hemp ash ceiling construction technology, but the overall weight is greatly reduced, which is lower than the weight of the ceiling constructed by modern technology in Example 1, and fully meets the requirements for the weight of the ceiling in the repair of ancient buildings.
[0057] 2. Overall quality According to the size of a 100 square meter building, the ceiling was made using the process of Examples 1 to 10 of the present application, and then the ceiling was made using the process of Comparative Examples 1 to 4. The ceilings of Examples 1 to 10 of the present application and the ceilings of Comparative Examples 1 to 4 were hung with a hanger. After the maintenance was completed, an ultrasonic flaw detection device was used to detect whether the outer plaster layer was cracked; then the ceiling was placed in a UV aging room, and under UV irradiation, the temperature in the aging room was maintained at 55°C and the humidity was 150%. The aging treatment was carried out for 120 days, and then the ultrasonic flaw detection device was used again to detect whether the outer plaster layer was cracked. The results are shown in Table 2.
[0058] Table 2 Overall quality test results of Examples 1 to 10 and Comparative Examples 1 to 4
[0059] It can be seen from the above test results that the ceiling construction processes of Examples 1 to 10 of the present application, after the specific design of the mortar ratio of the plastering, and under the premise of greatly reducing the thickness of the plastering layer, the ash layer did not crack after curing, and no obvious cracks appeared after aging treatment, which shows that the crack resistance of the ceiling plastering layer is very excellent; while the modern process of Comparative Example 1 and the traditional process of Comparative Example 2 both showed slight cracks in the outer layer after aging, which shows that their aging resistance is relatively weak.
[0060] By comparing the test results of Example 10 with those of Comparative Examples 3 to 4 in the above test results, it can be seen that after adding nano-silicon dioxide as a filler in the present application, the overall strength of the mortar has been significantly improved, and compared with Comparative Example 3 without adding nano-silicon dioxide, the crack resistance has been significantly enhanced. In addition, in the ceiling construction process of the present application, the middle ash layer uses polypropylene staple fibers instead of hemp knives, and after adding a small amount of polypropylene staple fibers and TPP tricresyl phosphate to the outer ash layer, the overall crack resistance of the plaster layer has been significantly improved, and the aging resistance is also very excellent. After adding polypropylene staple fibers, the mechanical properties, stability and anti-aging properties of the ash layer are all improved; and TPP tricresyl phosphate, as a compatibilizer, can not only promote the uniform dispersion of polypropylene staple fibers in the mortar, but also has certain anti-ultraviolet properties, which can effectively protect the plaster layer from ultraviolet aging.
[0061] Through the comparison of the test results of Examples 1 to 5 in the above test results, it can be seen that after the ratio of the first coat of ash, the second coat of ash and the covering ash of the present application is optimized, the overall quality of the ash layer will be further improved; after the thickness of each ash layer is optimized, the overall quality of the ash layer will also be further improved.
[0062] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A construction process for a reed foil and hemp ash ceiling, characterized in that: The following steps are involved: S1. Installation of wooden keels: The main keel wooden beams are arranged along the purlin direction, and the secondary keel wooden beams are arranged at intervals. The keel and the roof beam are fixed with wooden beams as hangers. The lower part of the left and right side beams is nailed to the side of the keel, and the upper part is nailed to the side of the purlin or beam. S2. Installation of hanging nails and reed foil: Fix the finished reed foil to the bottom of the wooden keel with nails. Use more reed foil during installation to ensure that the gap between reed foils is less than 5mm. Then, according to the arrangement of the wooden keel, use nails to wrap thin iron wire for tensioning and maintenance. S3, preparing mortar: preparing the first layer of mortar, the components of which include slaked lime, hemp knife, bluestone powder and nano-silicon dioxide; preparing the second layer of mortar, the components of which include slaked lime, polypropylene staple fiber, nano-silicon dioxide and compatibilizer; preparing the topcoat mortar, the topcoat mortar is prepared according to the weight ratio of slaked lime, hemp knife, polypropylene staple fiber and compatibilizer of 98:1~3:2~4:4~6; S4. Plastering: Use the first coat of plaster to construct a 2~4mm thick inner plaster layer on the outside of the reed foil, use the second coat of plaster to construct a 4~8mm thick middle plaster layer on the outside of the inner plaster layer, and finally use the finishing plaster to construct a 1~3mm thick outer plaster layer on the outside of the middle plaster layer. After the outer plaster layer is constructed, press it repeatedly to make the surface smooth and compact to complete the ceiling construction.
2. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S1, the size of the main keel wood beam is 100mm×60mm, the size of the secondary keel wood beam is 50mm×50mm, the size of the suspension rod wood beam is 70mm×70mm, the secondary keel spacing is 40mm, and the suspension rod spacing is 1000mm.
3. The construction process of the reed foil and hemp ash ceiling according to claim 2 is characterized in that: In step S2, when the length of the main keel is insufficient, it is overlapped on the side, the overlap length is not less than 50 cm, the overlap is fixed with nails, tied with wire, and a suspension rod is added at the overlap.
4. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S2, the nails are spaced 30 mm apart.
5. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S2, when the reed foil is installed, individual reeds are shortened in areas with high density, and areas with large gaps are reinforced with iron wire and a single reed.
6. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S3, the weight proportions of the components of the first layer of ash include: 90-100 parts of slaked lime, 4-6 parts of hemp knife, 3-5 parts of bluestone powder, and 6-10 parts of nano silicon dioxide.
7. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S3, the weight proportions of the components of the second layer of ash include: 90-100 parts of slaked lime, 4-6 parts of polypropylene staple fibers, 4-8 parts of nano-silicon dioxide, and 6-8 parts of TPP tricresyl phosphate.
8. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S4, the middle ash layer is constructed after the surface of the inner ash layer is 60% to 70% dry, and the middle ash layer needs to be pushed into the inner ash layer during construction.
9. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S4, after the middle ash layer is constructed, the surface needs to be smoothed, and then the texture is processed on the outside.
10. The construction process of the reed foil and hemp ash ceiling according to claim 1 is characterized in that: In step S4, the outer ash layer is constructed after the surface of the middle ash layer is 70% to 80% dry.