Preparation method of degradable firework base

By mixing tailings with porous ceramics, carboxymethylcellulose sodium and foaming agent and pressing the molding method, the problems of cumbersome materials and waste of resources in traditional firework bases are solved, and a stable and environmentally friendly degradable firework base is obtained. It has high compressive strength and suitable water absorption.

CN118896522AActive Publication Date: 2024-11-05HUNAN ZHONGZI TAILINGS NEW MATERIALS TECHNOLOGY RESEARCH INSTITUTE CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410794964.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-05
Estimated Expiration
2044-06-19

Smart Images

  • Figure CN118896522A_ABST
    Figure CN118896522A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a degradable firework base, and belongs to the technical field of firework production. The preparation method of the degradable firework base comprises the following steps that S1, tailings and first water are mixed to obtain first slurry; s2, mixing porous ceramic, sodium carboxymethyl cellulose and second water at 45-55 DEG C to obtain second slurry; s3, mixing the first slurry and the second slurry, and then adding a foaming agent for mixing to obtain third slurry; and S4, the third slurry is injected into a firework base mold for compression molding, and then the degradable firework base is obtained through maintenance. The prepared degradable firework base is stable in quality, excellent in compressive strength, appropriate in water absorption rate and low in dry density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fireworks production, and in particular to a method for preparing a degradable fireworks base. Background Art

[0002] Traditional combination fireworks base materials use paper as the main raw material. Large sheets of paper are cut into small paper patterns, which are then pasted layer by layer to a certain thickness and then manually or mechanically rolled into paper tubes of the required specifications. This traditional production process has many steps, low efficiency, and waste of materials, resulting in high production costs.

[0003] In the prior art, waste plastic is used as the main base material, and rice husk is added as filler, which is mixed in a rubber refining machine to form a block base material, and then pressed into a shell of the required specifications for a display shell. The base material can also be processed into a firework tube body. The waste plastic is a thermoplastic plastic and can be used as an adhesive mixed with the base material of the display shell. It has the advantages of light weight, high strength, beautiful appearance, not easy to deform, and no static electricity reflection. In addition, waste plastic and rice husk are used as base materials to turn waste into treasure, saving a large amount of paper materials for the fireworks industry. Although waste plastic and rice husk replace traditional paper, due to the difficulty in recycling and modifying waste plastic, the quality of the manufactured product is not stable enough, and there is a safety hazard.

[0004] At present, the mud produced during ore mining, namely tailings, is generally discarded and there is a waste of resources. How to make biodegradable fireworks bases with stable quality from tailings is a problem that the existing technology needs to solve. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned technical deficiencies, provide a method for preparing a degradable firework base, and solve the technical problem of how to make a degradable firework base with stable quality through tailings in the prior art.

[0006] In order to achieve the above technical objectives, the technical solution of the present invention provides a method for preparing a degradable firework base, comprising the following steps:

[0007] S1, mixing the tailings and the first water to obtain a first slurry;

[0008] S2, mixing the porous ceramic, sodium carboxymethyl cellulose and the second water at 45-55° C. to obtain a second slurry;

[0009] S3, mixing the first slurry and the second slurry, and then adding a foaming agent to obtain a third slurry;

[0010] S4, injecting the third slurry into the firework base mold for pressing and forming, and then curing to obtain the degradable firework base.

[0011] In any embodiment, the raw materials, calculated by weight of each raw material, include: 200-300 parts of tailings, 100-200 parts of first water, 30-50 parts of porous ceramics, 10-20 parts of sodium carboxymethyl cellulose, 10-20 parts of second water and 30-40 parts of foaming agent.

[0012] In any embodiment, the porous ceramic is a modified porous ceramic, and the modified porous ceramic is prepared by the following steps: mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, immersing porous alumina, porous silica and sepiolite in the mixed solution, filtering, and drying to obtain the modified porous ceramic.

[0013] In any embodiment, the mass ratio of the porous alumina, the porous silica and the sepiolite is 1:(2-3):(1-2).

[0014] In any embodiment, the mass ratio of the ethanol solution to the KH570 silane coupling agent is 10:(2-3), the volume concentration of the ethanol solution is 70-80%; the mass ratio of the porous alumina to the KH570 silane coupling agent is (2-3):(2-3).

[0015] In any embodiment, the immersion time is 30-60 minutes.

[0016] In any embodiment, the foaming agent is one or both of azodicarbonamide and calcium carbonate.

[0017] In any embodiment, the foaming agent is a mixture of azodicarbonamide and calcium carbonate; wherein the mass ratio of the azodicarbonamide to the calcium carbonate is 1:(2-4).

[0018] In any embodiment, in step S1, the particle size of the tailings is 100-150 mesh.

[0019] In any embodiment, in step S4, after forming, the base is dried in the shade for 4-6 hours to obtain the degradable firework base.

[0020] Compared with the prior art, the beneficial effects of the present invention include: firstly, the tailings and the first water are mixed to obtain the first slurry, and the porous ceramic, sodium carboxymethyl cellulose and the second water are mixed to obtain the second slurry. The porous ceramic and sodium carboxymethyl cellulose can absorb the sodium carboxymethyl cellulose through the porous material. Then, the first slurry and the second slurry are mixed. Under the action of sodium carboxymethyl cellulose, the porous ceramic and the tailings material form a pre-bonding force. Then, a foaming agent is added to mix to obtain a third slurry. The addition of the foaming agent facilitates the formation of pores in the third slurry to reduce the weight of the formed fireworks base and ensure the uniform distribution of the components. Then, the third slurry with more pores is further pressed and formed, and then cured to obtain the degradable fireworks base. The degradable fireworks base has stable quality, excellent compressive strength, relatively suitable water absorption rate and low dry density. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a photograph of the degradable oxidized base prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0023] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0024] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0025] This specific embodiment provides a method for preparing a degradable firework base, comprising the following steps:

[0026] S1, mixing the tailings and the first water to obtain a first slurry; the particle size of the tailings is 100-150 mesh;

[0027] S2, mixing the porous ceramic, sodium carboxymethyl cellulose and the second water at 45-55° C. to obtain a second slurry;

[0028] S3, mixing the first slurry and the second slurry, and then adding a foaming agent to obtain a third slurry;

[0029] S4, injecting the third slurry into the firework base mold and pressing it into shape, and then drying and curing it in the shade for 4-6 hours to obtain the degradable firework base.

[0030] In this specific embodiment, the raw materials, calculated according to the weight of each raw material, include: 200-300 parts of tailings, 100-200 parts of first water, 30-50 parts of porous ceramics, 10-20 parts of sodium carboxymethyl cellulose, 10-20 parts of second water and 30-40 parts of foaming agent; the foaming agent is one or both of azodicarbonamide and calcium carbonate.

[0031] In some embodiments, the porous ceramic is a modified porous ceramic, which is prepared by the following steps: mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, placing porous alumina, porous silica and sepiolite in the mixed solution and immersing for 30-60 minutes, then filtering, and then drying to obtain the modified porous ceramic; the mass ratio of the porous alumina, the porous silica and the sepiolite is 1:(2-3):(1-2); the mass ratio of the ethanol solution and the KH570 silane coupling agent is 10:(2-3), and the volume concentration of the ethanol solution is 70-80%; the mass ratio of the porous alumina to the KH570 silane coupling agent is (2-3):(2-3). The modified porous ceramics are loaded with KH570 silane coupling agent, which can effectively combine with sodium carboxymethyl cellulose to improve its binding force, thereby improving the binding force between the porous ceramics and the tailings, improving its strength, and then under the action of the foaming agent, it can also ensure that the final degradable firework base has a higher strength.

[0032] In some preferred embodiments, the foaming agent is a mixture of azodicarbonamide and calcium carbonate; wherein the mass ratio of azodicarbonamide to calcium carbonate is 1:(2-4). The foaming agent used in combination with the two is more conducive to improving the strength of the firework base, which may be due to the fact that calcium carbonate itself has a certain load effect, and the loading of azodicarbonamide synergistically foams, resulting in a better foaming effect, thereby promoting the uniform distribution of each component and improving the strength.

[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0034] In the present invention, reference is made to “some embodiments”, “this embodiment”, examples, etc., which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0035] If similar descriptions of "first / second" appear in the application documents, the following instructions are added. In the following description, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged in a specific order or sequence where permitted, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein.

[0036] In this embodiment, the term "and / or" is merely a description of the association relationship between associated objects, indicating that three relationships may exist. For example, object A and / or object B may represent three situations: object A exists alone, object A and object B exist at the same time, and object B exists alone.

[0037] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer, and are all conventional products that can be obtained commercially, and the related equipment is the general equipment of the prior art.

[0038] The tailings in the following examples are lithium tailings.

[0039] It should be noted that, during the preparation process, 1 part of each component is determined according to the weighing amount required by the test, and 1 part can represent 1g, 10g, 500, 1kg, 10kg or 50kg, etc., and the present invention is not limited to this.

[0040] Example 1

[0041] This embodiment provides a method for preparing a degradable firework base, comprising the following steps:

[0042] S1, stirring and mixing the lithium tailings and the first water to obtain a first slurry; the particle size of the lithium tailings is 100-150 mesh;

[0043] S2, stirring and mixing the porous ceramic, sodium carboxymethyl cellulose and the second water at 45° C. to obtain a second slurry;

[0044] S3, stirring and mixing the first slurry and the second slurry, and then adding a foaming agent and stirring and mixing to obtain a third slurry;

[0045] S4, injecting the third slurry into the firework base mold and pressing it into shape, and then drying and curing it in the shade for 4 hours to obtain the degradable firework base.

[0046] In this embodiment, the raw materials, calculated according to the weight of each raw material, include: 200 parts of lithium tailings, 150 parts of first water, 30 parts of porous ceramics, 15 parts of sodium carboxymethyl cellulose, 15 parts of second water and 35 parts of calcium carbonate.

[0047] In this embodiment, the porous ceramic is a modified porous ceramic, and the modified porous ceramic is prepared by the following steps: stirring and mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, placing porous alumina, porous silica and sepiolite in the mixed solution and immersing for 40 minutes, then filtering, and then drying to obtain the modified porous ceramic; the mass ratio of the porous alumina, the porous silica and the sepiolite is 1:2:1; the mass ratio of the ethanol solution and the KH570 silane coupling agent is 5:1, and the volume concentration of the ethanol solution is 70%; the mass ratio of the porous alumina to the KH570 silane coupling agent is 2:3.

[0048] Figure 1 This is a photo of the degradable firework base prepared in this embodiment. From the photo, it can be seen that the base has a uniform appearance, few flaws, and is strong.

[0049] Example 2

[0050] This embodiment provides a method for preparing a degradable firework base, comprising the following steps:

[0051] S1, stirring and mixing the lithium tailings and the first water to obtain a first slurry; the particle size of the lithium tailings is 100-150 mesh;

[0052] S2, stirring and mixing the porous ceramic, sodium carboxymethyl cellulose and the second water at 50° C. to obtain a second slurry;

[0053] S3, stirring and mixing the first slurry and the second slurry, and then adding a foaming agent and stirring and mixing to obtain a third slurry;

[0054] S4, injecting the third slurry into the firework base mold and pressing it into shape, and then drying and curing it in the shade for 6 hours to obtain the degradable firework base.

[0055] In this embodiment, the raw materials, calculated according to the weight of each raw material, include: 250 parts of lithium tailings, 200 parts of first water, 40 parts of porous ceramics, 15 parts of sodium carboxymethyl cellulose, 15 parts of second water and 35 parts of foaming agent; the foaming agent is a mixture of azodicarbonamide and calcium carbonate; wherein the mass ratio of the azodicarbonamide to the calcium carbonate is 1:3.

[0056] In this embodiment, the porous ceramic is a modified porous ceramic, and the modified porous ceramic is prepared by the following steps: stirring and mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, placing porous alumina, porous silica and sepiolite in the mixed solution and immersing for 50 minutes, then filtering, and then drying to obtain the modified porous ceramic; the mass ratio of the porous alumina, the porous silica and the sepiolite is 1:3:2; the mass ratio of the ethanol solution and the KH570 silane coupling agent is 10:3, and the volume concentration of the ethanol solution is 75%; the mass ratio of the porous alumina to the KH570 silane coupling agent is 3:2.

[0057] Example 3

[0058] This embodiment provides a method for preparing a degradable firework base, comprising the following steps:

[0059] S1, stirring and mixing the lithium tailings and the first water to obtain a first slurry; the particle size of the lithium tailings is 100-150 mesh;

[0060] S2, stirring and mixing the porous ceramic, sodium carboxymethyl cellulose and the second water at 50° C. to obtain a second slurry;

[0061] S3, stirring and mixing the first slurry and the second slurry, and then adding a foaming agent and stirring and mixing to obtain a third slurry;

[0062] S4, injecting the third slurry into the firework base mold and pressing it into shape, and then drying and curing it in the shade for 5 hours to obtain the degradable firework base.

[0063] In this embodiment, the raw materials, calculated according to the weight of each raw material, include: 300 parts of lithium tailings, 100 parts of first water, 40 parts of porous ceramics, 10 parts of sodium carboxymethyl cellulose, 20 parts of second water and 40 parts of foaming agent; the foaming agent is a mixture of azodicarbonamide and calcium carbonate; wherein the mass ratio of the azodicarbonamide to the calcium carbonate is 1:2.

[0064] In this embodiment, the porous ceramic is a modified porous ceramic, and the modified porous ceramic is prepared by the following steps: stirring and mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, placing porous alumina, porous silica and sepiolite in the mixed solution and immersing for 60 minutes, then filtering, and then drying to obtain the modified porous ceramic; the mass ratio of the porous alumina, the porous silica and the sepiolite is 1:2:2; the mass ratio of the ethanol solution and the KH570 silane coupling agent is 10:2.5, and the volume concentration of the ethanol solution is 75%; the mass ratio of the porous alumina to the KH570 silane coupling agent is 2:3.

[0065] Example 4

[0066] This embodiment provides a method for preparing a degradable firework base, comprising the following steps:

[0067] S1, stirring and mixing the lithium tailings and the first water to obtain a first slurry; the particle size of the lithium tailings is 100-150 mesh;

[0068] S2, stirring and mixing the porous ceramic, sodium carboxymethyl cellulose and the second water at 55° C. to obtain a second slurry;

[0069] S3, stirring and mixing the first slurry and the second slurry, and then adding a foaming agent and stirring and mixing to obtain a third slurry;

[0070] S4, injecting the third slurry into the firework base mold and pressing it into shape, and then drying and curing it in the shade for 5 hours to obtain the degradable firework base.

[0071] In this embodiment, the raw materials, calculated according to the weight of each raw material, include: 300 parts of lithium tailings, 100 parts of first water, 50 parts of porous ceramics, 20 parts of sodium carboxymethyl cellulose, 10 parts of second water and 30 parts of foaming agent; the foaming agent is a mixture of azodicarbonamide and calcium carbonate; wherein the mass ratio of the azodicarbonamide to the calcium carbonate is 1:4.

[0072] In this embodiment, the porous ceramic is a modified porous ceramic, and the modified porous ceramic is prepared by the following steps: stirring and mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, placing porous alumina, porous silica and sepiolite in the mixed solution and immersing for 30 minutes, then filtering, and then drying to obtain the modified porous ceramic; the mass ratio of the porous alumina, the porous silica and the sepiolite is 1:2:1; the mass ratio of the ethanol solution and the KH570 silane coupling agent is 10:3, and the volume concentration of the ethanol solution is 80%; the mass ratio of the porous alumina to the KH570 silane coupling agent is 3:2.

[0073] Example 5

[0074] The only difference between this embodiment and embodiment 1 is that the foaming agent is azodicarbonamide, and the other preparation methods and raw material dosages are the same as those in embodiment 1.

[0075] Comparative Example 1

[0076] The only difference between this comparative example and Example 2 is that the porous ceramics are unmodified porous alumina, porous silica and sepiolite in the same amount as in Example 2.

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 2 is that the order of adding the foaming agent is different, which is as follows:

[0079] This comparative example proposes a method for preparing a degradable firework base, comprising the following steps:

[0080] S1, stirring and mixing the lithium tailings and the first water, and then adding a foaming agent and stirring and mixing to obtain a first slurry; the particle size of the lithium tailings is 100-150 mesh;

[0081] S2, stirring and mixing the porous ceramic, sodium carboxymethyl cellulose and the second water at 50° C. to obtain a second slurry;

[0082] S3, stirring and mixing the first slurry and the second slurry, and then adding a foaming agent and stirring and mixing to obtain a third slurry;

[0083] S4, injecting the third slurry into the firework base mold and pressing it into shape, and then drying and curing it in the shade for 6 hours to obtain the degradable firework base.

[0084] The addition amount of each component and dosage are the same as those in Example 2.

[0085] Comparative Example 3

[0086] The difference between this comparative example and Example 2 is that the materials are not added in order, but all the amounts are mixed and stirred at the same time to obtain a mixed slurry, which is then injected into a firework base mold for pressing and forming, and then dried in the shade for 6 hours to obtain the degradable firework base.

[0087] The compressive strength, water absorption rate and dry density of the degradable firework bases prepared in Examples 1-4 and Comparative Examples 1-3 were tested, and the results are shown in Table 1. Water absorption rate test: The degradable firework base was completely immersed in water for 24 hours, and then the base was taken out to dry the surface moisture in the shade, and the water absorption rate of the base was obtained by weighing the mass difference of the base before and after immersion.

[0088] Comparative Example 4

[0089] The difference between this comparative example and Example 2 is that the raw material for making the modified porous ceramic does not use sepiolite, and the preparation method, raw materials and dosage of other degradable firework bases are the same as those in Example 2. Specifically, the porous ceramic is a modified porous ceramic, and the modified porous ceramic is prepared by the following steps: stirring and mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, placing porous alumina and porous silica in the mixed solution and immersing for 50 minutes, then filtering, and then drying to obtain the modified porous ceramic; the dosage of the porous alumina and the porous silica is the same as that in Example 2, and the dosage of sepiolite is compensated by part of the porous alumina and part of the porous silica, and the sum of the mass of the supplemented porous alumina and porous silica is the mass of the sepiolite.

[0090] Table 1 Compressive strength, water absorption and dry density of the degradable firework bases prepared in Examples 1-4 and Comparative Examples 1-3

[0091]

[0092]

[0093] It can be seen from Table 1 that when only azodicarbonamide or calcium carbonate is used as the foaming agent in Example 1 and Example 5, the compressive strength of the degradable firework base obtained is poor, while when the two are mixed, the compressive strength of the degradable firework base obtained is higher. This may be because the combination of the two can improve the uniformity of the components in the slurry, thereby improving its compressive strength.

[0094] The compressive strength of comparative example 1 is low, the water absorption rate is low and the dry density is high. This may be because the unmodified porous alumina, porous silica and sepiolite do not carry coupling agents, resulting in relatively poor binding force between them and sodium carboxymethyl cellulose, and then poor binding force with tailings. The binding force is more easily weakened under the action of the foaming agent, which leads to the problem of uneven distribution of components, which in turn affects the foaming effect, resulting in low compressive strength, low water absorption rate and high dry density.

[0095] The main reason for the higher dry density of Comparative Example 2 is that the foaming agent is added too early, resulting in poor foaming effect and high dense dry density of the material.

[0096] When the comparative example 3 is mixed together, the components are difficult to be evenly distributed, and thus the compressive strength is poor.

[0097] In the case of lack of sepiolite, the strength of comparative example 4 becomes worse. This may be because the sepiolite in the present invention absorbs water and softens, and the combination with tailings through sodium carboxymethyl cellulose can significantly improve the mutual binding force of each component, and hardens after drying, thereby significantly improving the strength.

[0098] The degradable firework base proposed by the present invention has a certain moisture-proof effect, is fire-resistant, and has high strength. The appropriate water absorption rate ensures that it has a certain moisture-proof effect and can be degraded into powder in nature.

[0099] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a degradable firework base, characterized in that: The following steps are involved: S1, mixing the tailings and the first water to obtain a first slurry; S2, mixing the porous ceramic, sodium carboxymethyl cellulose and second water at 45-55° C. to obtain a second slurry; S3, mixing the first slurry and the second slurry, and then adding a foaming agent to obtain a third slurry; S4, injecting the third slurry into the firework base mold for pressing and forming, and then curing to obtain the degradable firework base.

2. The method for preparing a degradable firework base according to claim 1, characterized in that: The raw materials include, by weight of each raw material, 200-300 parts of tailings, 100-200 parts of first water, 30-50 parts of porous ceramics, 10-20 parts of sodium carboxymethyl cellulose, 10-20 parts of second water and 30-40 parts of foaming agent.

3. The method for preparing the degradable firework base according to claim 2, characterized in that: The porous ceramic is a modified porous ceramic, which is prepared by the following steps: mixing an ethanol solution and a KH570 silane coupling agent to obtain a mixed solution, immersing porous alumina, porous silica and sepiolite in the mixed solution, filtering, and drying to obtain the modified porous ceramic.

4. The method for preparing the degradable firework base according to claim 3, characterized in that: The mass ratio of the porous alumina, the porous silica and the sepiolite is 1:(2-3):(1-2).

5. The method for preparing a degradable firework base according to claim 4, characterized in that: The mass ratio of the ethanol solution to the KH570 silane coupling agent is 10:(2-3), and the volume concentration of the ethanol solution is 70-80%; the mass ratio of the porous alumina to the KH570 silane coupling agent is (2-3):(2-3).

6. The method for preparing a degradable firework base according to claim 3, characterized in that: The immersion time is 30-60 minutes.

7. The method for preparing a degradable firework base according to claim 1 or 2, characterized in that: The foaming agent is one or both of azodicarbonamide and calcium carbonate.

8. The method for preparing a degradable firework base according to claim 7, characterized in that: The foaming agent is a mixture of azodicarbonamide and calcium carbonate; wherein the mass ratio of the azodicarbonamide to the calcium carbonate is 1:(2-4).

9. The method for preparing a degradable firework base according to claim 1 or 2, characterized in that: In step S1, the particle size of the tailings is 100-150 mesh.

10. The method for preparing a degradable firework base according to claim 1 or 2, characterized in that: In step S4, after forming, the base is dried in the shade for 4-6 hours to obtain the degradable firework base.

Citation Information

Patent Citations

  • Firework set-off barrel and manufacturing method thereof

    CN103787619A

  • Granite waste stone dust foam ceramics and preparation method thereof

    CN107586102A

  • Lightweight, high-strength and high-toughness foamed ceramic decorative integrated board and production method thereof

    CN109291549A

  • Method for preparing lightweight wallboard from kaolin tailing slag

    CN110357580A

  • Preparation method of tailing-based porous ceramic material

    CN115677377A