Flame-retardant composite current collector and preparation method thereof

By adopting a composite fluid design of a reversible phase change flame retardant layer and a conductive layer in lithium-ion batteries, the problem of thermal runaway in lithium-ion batteries is solved, and the stable heat dissipation and flame retardant effects are achieved, and the safety of the battery is improved. .

CN118899448APending Publication Date: 2024-11-05JIANGSU THREE LAYERS TECH CO LTD

Patent Information

Application Number
CN202410984962.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Lithium-ion batteries are prone to thermal runaway under abnormal conditions such as external short circuit or needle puncture, resulting in combustion and explosion. The conductive and thermal conductivity of existing current collectors exacerbate this risk in high temperature environments.

Method used

A flame retardant composite fluid is adopted, including a substrate layer, a phase change flame retardant layer and a conductive layer. The phase change flame retardant layer is converted from an insulating phase to a metal phase under an environment of 60°C-80°C, and is reversible at high temperatures. , combined with the design of the conductive layer to improve density and flame retardant properties.

Benefits of technology

Maintain heat dissipation stability in high temperature environments and significantly improve flame retardant effect, avoid thermal runaway, and enhance battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899448A_ABST
    Figure CN118899448A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of current collectors, in particular to a flame-retardant composite current collector and a preparation method thereof. A phase-change flame-retardant layer and a conductive layer are sequentially arranged on the two sides of the base material layer; wherein the phase-change flame-retardant layer is subjected to reversible phase change from an insulating phase to a metal phase in an environment of 60-80 DEG C after absorbing heat; according to the flame-retardant composite current collector and the preparation method thereof, the phase-change flame-retardant layer which can absorb heat in an environment of 60-80 DEG C and is converted from an insulating phase to a metal phase is arranged, so that the density of the composite current collector can be maintained and further improved, and meanwhile, reversible conversion from an insulator to metal can occur in a high-temperature environment; the heat dissipation stability of normal work of the current collector is guaranteed, and a good flame retardant effect is achieved under the condition of sudden high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of current collectors, and in particular to a flame retardant composite current collector and a preparation method thereof. Background Art

[0002] When lithium-ion batteries encounter extreme physical disturbances such as external short circuits or needle punctures, their internal reaction mechanisms will be significantly unbalanced, resulting in a violent and uncontrollable energy release process, the so-called "thermal runaway" phenomenon. Under such fault conditions, the chemical reaction rate inside the battery soars sharply, accompanied by a large amount of heat energy generation. This heat cannot be effectively channeled and dissipated, forming high-temperature hot spots inside the battery, which continue to accumulate and aggravate local temperature rise, eventually breaking through the thermal stability threshold of the battery material and inducing a series of serious safety issues.

[0003] In lithium-ion battery systems, the current collector is a key component that connects the active material to the external circuit. The electrical and thermal conductivity of the current collector directly affects the overall performance and safety characteristics of the battery. The current collector is usually made of metal materials with good electrical and thermal conductivity (such as aluminum, copper, etc.) to ensure the effective transmission of charge and the effective evacuation of heat. However, when the battery faces abnormal operating conditions such as external short circuit or acupuncture, the efficient electrical conductivity of the current collector may become an important factor in accelerating the thermal runaway process. At this time, the current collector quickly conducts the heat generated by the short-circuit current or local violent reaction, which accelerates the diffusion of heat inside the battery, rapidly expands the high-temperature area, and increases the risk of thermal runaway. At the same time, the good thermal conductivity of the current collector may also cause the heat to be quickly transferred to other parts of the battery, such as the contact interface between the electrode and the diaphragm, the battery casing, etc. If these parts fail due to excessive thermal stress, it will further increase the safety risk of the battery.

[0004] In summary, when lithium-ion batteries encounter abnormal conditions such as external short circuits or needle punctures, they will experience thermal runaway due to intense internal heat generation, which can lead to serious safety issues such as combustion and explosion. In this process, the current collector, as an efficient electrical and thermal conductor inside the battery, has fast electrical and thermal conductivity under abnormal conditions, which is beneficial to improving battery performance during normal operation, but when the battery is on the edge of danger, it may accelerate the process of thermal runaway and increase safety hazards.

[0005] Therefore, how to avoid thermal runaway of the current collector under high temperature conditions is a technical problem that urgently needs technology in this field. Summary of the invention

[0006] The present invention provides a flame retardant composite current collector and a preparation method thereof, so as to solve the problem that thermal runaway is prone to occur in the existing current collector under high temperature environment.

[0007] In order to solve the above technical problems, the present invention provides a flame retardant composite current collector, comprising: a substrate layer; a phase change flame retardant layer and a conductive layer are sequentially arranged on both sides of the substrate layer; wherein the phase change flame retardant layer undergoes a reversible phase change from an insulating phase to a metallic phase under an environment of 60°C-80°C after absorbing heat.

[0008] Furthermore, the phase change flame retardant layer includes any one or more combinations of VO2, V3O7 and V2O5.

[0009] Furthermore, the phase change flame retardant layer also includes a combination of any one or more of VO2, V3O7 and V2O5 doped with metal elements; wherein the metal elements include a combination of any one or more of Ge, Nb, Mo, W, Ta, Ti, Al, Ga and Cr.

[0010] Furthermore, the insulating phase in the phase-change flame-retardant layer is specifically a low-temperature monoclinic structure, and the metal phase is specifically a high-temperature tetragonal structure.

[0011] Furthermore, the thickness of the phase change flame retardant layer is 5nm-100nm.

[0012] Furthermore, the substrate layer includes any one of a biaxially oriented polypropylene film, a cast polypropylene film, a polyethylene terephthalate film, a polyimide film and a polyethylene naphthalate film.

[0013] Furthermore, the thickness of the substrate layer is 3 μm-20 μm.

[0014] Furthermore, the conductive layer includes any one or more combinations of aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten and stainless steel.

[0015] Furthermore, the single layer thickness of the conductive layer is 500nm-5μm.

[0016] On the other hand, the present invention also provides a method for preparing the flame-retardant composite current collector as described above, comprising the following steps: step S1, performing surface cleaning pretreatment on the substrate layer; step S2, using any one of evaporation, sputtering, and CVD methods to deposit a phase change flame retardant layer on the substrate layer; step S3, using any one of evaporation, sputtering, and CVD methods to deposit a conductive layer on the phase change flame retardant layer; and step S4, repeating steps S2 and S3 on the other side of the substrate layer to obtain a flame retardant composite current collector.

[0017] The beneficial effect of the present invention is that the flame-retardant composite current collector and its preparation method of the present invention, by providing a phase change flame-retardant layer that can absorb heat and transform from an insulating phase to a metallic phase under a temperature of 60-80°C, can maintain and further improve the density of the composite current collector while allowing a reversible transformation from metal to insulator to occur under a high temperature environment, thereby ensuring the heat dissipation stability of the normal operation of the current collector and achieving a good flame retardant effect under sudden high temperature conditions.

[0018] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and the drawings.

[0019] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 The schematic diagrams of the structures of the flame-retardant composite current collectors involved in some embodiments are shown.

[0022] In the figure:

[0023] 1. Base material layer; 2. Phase change flame retardant layer; 3. Conductive layer. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Under external short-circuit conditions, the resistance between the positive and negative electrodes of the battery instantly drops to an extremely low level, causing a large current to flow abnormally in a very short time, generating a large amount of Joule heat; and in the needle puncture experiment, sharp objects penetrate the battery casing and internal components, directly destroying the original electrochemical environment inside the battery, triggering a local violent reaction and quickly generating a large amount of heat. In either case, the sharp increase in temperature inside the battery may not only cause overheating and decomposition of the electrolyte, releasing flammable gases, but even worse, it will trigger a thermochemical reaction between the positive active material and the electrolyte, forming an exothermic chain reaction, further exacerbating heat accumulation. Once this vicious cycle is formed, the internal pressure of the battery increases sharply. If it exceeds the tolerance limit of the packaging material, it may cause the battery casing to rupture, releasing high-temperature gases and flames, causing the battery to burn or even explode, posing a serious safety threat to the surrounding environment and personnel.

[0026] As an indispensable component of the battery, the current collector plays an extremely important role, and its performance cannot be ignored in the overall battery performance. The traditional metal foil current collector affects the energy density of the battery due to the presence of a thick metal layer. Compared with metal materials, polymer materials have lower density and higher mechanical strength, so the use of polymer materials is expected to make a breakthrough in the energy density of the battery.

[0027] In the prior art, taking Chinese patent document CN218677203U as an example, a hole structure design is adopted to cleverly embed the flame retardant structure inside the composite current collector. This strategy aims to activate and release the flame retardant in the hole under high temperature when the composite current collector encounters a fire, thereby forming an effective flame retardant barrier, inhibiting the spread of flames and heat transfer, and ensuring the flame retardancy of the overall structure.

[0028] At the same time, another widely used technical route is to directly attach the flame retardant components to the surface of the current collector through a coating process to form a protective layer enriched with flame retardant components. This method aims to build the first line of defense, that is, before the external heat source directly contacts the current collector, the surface coating absorbs heat, releases smoke suppression substances or produces a heat insulation barrier to delay or prevent the current collector from being heated to the ignition point. In addition, there is a strategy to introduce flame retardants during the preparation of the base film, and evenly disperse them inside the base film through blending and modification, giving it inherent flame retardant properties from the material body level.

[0029] Although the above technical solutions have improved the flame retardant properties of composite current collectors at different levels, they all face some inherent limitations. These limitations are particularly prominent when dealing with sudden fire events such as thermal runaway, especially thermal runaway caused by short circuits in battery systems. Thermal runaway caused by short circuits is usually a gradual temperature rise process. The local temperature rises sharply in the initial stage, but it has not yet triggered a large area of ​​base film combustion. However, most existing flame retardant configurations, especially those filled flame retardants buried deep inside the base film, are often unable to quickly and directly release their flame retardant properties in the initial stage of heat source action due to the physical barrier limitations of the base film material. The effective release of these flame retardants often depends on the pyrolysis, melting or even rupture of the base film material after reaching a certain temperature. This process has a significant time lag, which may result in the failure to suppress the development of the fire in a timely manner in the critical early stages.

[0030] In addition, short circuits often occur in local locations of the battery system, where the heat is concentrated and intense in a short period of time, and the demand for flame retardants is highly spatially and temporally concentrated. However, since most of the flame retardants are sealed inside the base film, the part that can effectively participate in the fire extinguishing reaction at the initial stage of the short circuit is limited to the small amount of flame retardants released by the surrounding exposed or ruptured areas, which undoubtedly limits the utilization efficiency of flame retardants at critical moments and reduces emergency response capabilities.

[0031] As for the application of flame retardants by coating, although it can form immediate protection on the surface of the current collector, it is not without disadvantages. On the one hand, the presence of the coating may have an adverse effect on the bonding strength between the subsequent current collector and the metal layer, especially under high temperature conditions. If the thermal stability and compatibility of the flame retardant coating with the metal layer are not ideal, it may cause bonding failure and affect the overall mechanical stability and electrochemical performance of the battery. On the other hand, although the coating method is more conducive to the direct release of flame retardants than internal filling, in actual applications, the release of flame retardants may still be insufficient or untimely, especially in the face of local high-temperature heat sources. The coating may crack or fall off due to uneven heat conduction or concentrated thermal stress, which hinders the effective use of flame retardants.

[0032] Therefore, although the flame retardant technologies of existing composite current collectors have their own characteristics and advantages, there are still certain lags and limitations in the immediate flame retardant response and efficient use of flame retardants in response to rapid temperature rise situations such as short circuits. In particular, the release control of internal filling flame retardants and the impact of coating flame retardants on the stability of composite structures are key links that need to be optimized in future technology research and development.

[0033] like Figure 1As shown, at least one embodiment provides a flame retardant composite current collector, including: a substrate layer; a phase change flame retardant layer and a conductive layer are sequentially arranged on both sides of the substrate layer; wherein the phase change flame retardant layer undergoes a reversible phase change from an insulating phase to a metallic phase under an environment of 60°C-80°C after absorbing heat.

[0034] In some embodiments, the phase change flame retardant layer includes any one or more combinations of VO2, V3O7 and V2O5. VO2 undergoes a reversible phase change from a low-temperature monoclinic insulating phase to a high-temperature tetragonal metallic phase at around 68°C. Due to its thermochromic properties, it can transform from an insulator to a metal when the external temperature changes, thereby achieving a flame retardant effect of the current collector.

[0035] In some embodiments, the phase change flame retardant layer further comprises a combination of any one or more of VO2, V3O7 and V2O5 doped with metal elements; wherein the metal elements comprise a combination of any one or more of Ge, Nb, Mo, W, Ta, Ti, Al, Ga and Cr.

[0036] In some embodiments, the phase change temperature and flame retardant modulation capability of phase change materials such as VO2, V3O7 and V2O5 can be changed by doping with other metal elements.

[0037] In some embodiments, the insulating phase in the phase-change flame-retardant layer is specifically a low-temperature monoclinic insulating structure, and the metal phase is specifically a high-temperature tetragonal metal structure. Taking vanadium dioxide (VO2) as an example, the monoclinic insulating structure it presents at low temperatures has an extremely high thermal resistance value, which means that heat is difficult to transfer through this phase, and can play a good role in preventing heat transfer in the early stage of thermal runaway.

[0038] In some embodiments, the thickness of the phase change flame retardant layer is 5 nm-100 nm, and can be 5 nm, 10 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 50 nm, 80 nm and 100 nm.

[0039] In some embodiments, the substrate layer includes any one of a biaxially oriented polypropylene film (OPP), a cast polypropylene film (CPP), a polyethylene terephthalate film (PET), a polyimide film (PI) and a polyethylene naphthalate film (PEN).

[0040] In some embodiments, the thickness of the substrate layer is 3 μm-20 μm, and can be 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm and 20 μm.

[0041] In some embodiments, the conductive layer includes any one or more of aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten and stainless steel.

[0042] In some embodiments, the single layer thickness of the conductive layer is 500 nm-5 μm, and can be 500 nm, 800 nm, 1 μm, 2 μm, 3 μm, 4 μm and 5 μm.

[0043] In some embodiments, the phase change flame retardant layer and the conductive layer are preferably formed using processes such as evaporation, sputtering, and CVD. Since the uniformity of the film formed by sputtering is better than that formed by evaporation, water electroplating, etc., sputtering is preferred when forming a film on a large substrate; the sputtering method can use alternating current (AC) magnetron sputtering, direct current (DC) magnetron sputtering, and radio frequency (RF) magnetron sputtering. Since the conductive layer is a conductor, direct current (DC) magnetron sputtering is preferred.

[0044] Preliminary preparation: In the chamber of the winding magnetron sputtering coating machine, place the processed flexible substrate on the unwinding roller of the unwinding chamber and wind it onto the winding roller; at the same time, place the required targets Z1 and Z2 on the cathode target positions corresponding to chambers C1 and C2 in turn. Chambers C1 and C2 are coating chambers, and the distance from the target to the substrate surface is adjusted to 10 cm; close all chamber doors, turn on the fore pump and molecular pump in turn, and wait until the vacuum degree of the chamber reaches 5×10 -4 When the pressure drops to 0.05 Pa, fill in process gas until the process vacuum is reached, open the cathode and drive roller to start coating, and control the winding speed at 5-12 m / min.

[0045] Step S1: Pre-treatment of the substrate surface by cleaning

[0046] Argon gas was introduced into the vacuum chamber, and the argon gas was ionized by providing 800 W of power to the ion source, thereby cleaning the surface of the substrate.

[0047] Step S2: Depositing a phase change flame retardant layer on the substrate layer

[0048] Sputtering gases argon and oxygen with a purity of not less than 99.99% are introduced into chamber C1, the argon amount is 400sccm, the oxygen amount is 50-200sccm, and the chamber pressure is stabilized at 0.3Pa. A phase change flame retardant layer of a certain thickness is formed on the base film using the Z1 target material through a dual rotating cathode and DC magnetron sputtering method. The composition is an oxide generated by the reaction of the sputtering target Z1 target material with oxygen; the dual rotating cathode and DC magnetron sputtering power is 1Kw-15Kw.

[0049] Step S3: Depositing a conductive layer on the phase change flame retardant layer

[0050] After the phase change flame retardant layer is generated, sputtering gas argon with a purity of not less than 99.99% is introduced into chamber C2, the argon amount is 300sccm, and the chamber pressure is stabilized at 0.3Pa. Through the dual rotating cathode and DC magnetron sputtering, a conductive layer of a certain thickness is formed on the film phase change flame retardant layer using the Z2 target material. The composition of the conductive layer is the same as the structural material of the sputtering target Z2 target material; the dual rotating cathode and DC magnetron sputtering power is 5Kw~50Kw.

[0051] Step S4: Repeat steps S2 and S3 on the other side of the substrate layer to obtain a flame retardant composite current collector.

[0052] In some embodiments, the parameters and performances of Examples 1-9 and Comparative Examples 1-2 are shown in Table 1 below, wherein Comparative Example 1 uses a traditional electrolytic copper foil with a thickness of 6 um, and Comparative Example 2 is a structure without a phase change flame retardant layer.

[0053] Table 1

[0054]

[0055] In some embodiments, the method of the extrusion test is specifically as follows: charging to 4.45V at a constant current of 0.5C at room temperature (25°C±3°C), and further charging the current to 0.05C at a constant voltage of 4.45V to make it fully charged, and then performing a screw extrusion test on the lithium-ion battery provided with the current collector of the corresponding embodiment, using a screw made of carbon steel with a size of M2*4*3.5mm, placed at the geometric center of the battery plane, and pressing the screw into the battery at a downward speed of 15mm / s and a pressure of 13KN±1KN, to observe whether the lithium-ion battery catches fire or explodes. If not, it is considered that the lithium-ion battery has passed the screw extrusion test.

[0056] In some embodiments, the impact test method is specifically as follows: Place a lithium-ion battery provided with a current collector of the corresponding embodiment on a plane. Place a rod with a diameter of 15.8 mm crosswise at the center of the sample. Drop a 9.1 kg weight from a height of 610 mm onto the sample. Each sample battery can only withstand one impact, and each test must be conducted using different samples according to regulations. The battery is qualified if it does not catch fire or explode.

[0057] In summary, the flame-retardant composite current collector and its preparation method are provided with a phase change flame-retardant layer that can absorb heat and transform from an insulating phase to a metallic phase under a temperature of 60-80°C. While being able to maintain and further improve the density of the composite current collector, a reversible transformation from metal to insulator can occur under a high temperature environment, which not only ensures the heat dissipation stability of the normal operation of the current collector, but also has a good flame retardant effect under sudden high temperature conditions.

[0058] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A flame retardant composite current collector, characterized in that: include: substrate layer; A phase-change flame-retardant layer and a conductive layer are sequentially arranged on both sides of the substrate layer; After absorbing heat, the phase-change flame-retardant layer undergoes a reversible phase change from an insulating phase to a metallic phase in an environment of 60° C. to 80° C.

2. The flame-retardant composite current collector according to claim 1, characterized in that: The phase-change flame-retardant layer includes any one or more combinations of VO2, V3O7 and V2O5.

3. The flame-retardant composite current collector according to claim 2, characterized in that: The phase-change flame-retardant layer further comprises any one or more combinations of VO2, V3O7 and V2O5 doped with metal elements; The metal elements include any one or more combinations of Ge, Nb, Mo, W, Ta, Ti, Al, Ga and Cr.

4. The flame-retardant composite current collector according to claim 1, characterized in that: The insulating phase in the phase-change flame-retardant layer is specifically a low-temperature monoclinic structure, and the metal phase is specifically a high-temperature tetragonal structure.

5. The flame-retardant composite current collector according to claim 1, characterized in that: The thickness of the phase-change flame-retardant layer is 5nm-100nm.

6. The flame-retardant composite current collector according to claim 1, characterized in that: The substrate layer includes any one of a biaxially oriented polypropylene film, a cast polypropylene film, a polyethylene terephthalate film, a polyimide film and a polyethylene naphthalate film.

7. The flame-retardant composite current collector according to claim 1, characterized in that: The thickness of the substrate layer is 3 μm-20 μm.

8. The flame-retardant composite current collector according to claim 1, characterized in that: The conductive layer includes any one or more combinations of aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten and stainless steel.

9. The flame-retardant composite current collector according to claim 1, characterized in that: The single layer thickness of the conductive layer is 500nm-5μm.

10. A method for preparing a flame retardant composite current collector according to any one of claims 1 to 9, characterized in that: The steps include: Step S1, performing surface cleaning pretreatment on the substrate layer; Step S2, depositing a phase change flame retardant layer on the substrate layer by any one of evaporation method, sputtering method and CVD method; Step S3, depositing a conductive layer on the phase change flame retardant layer by any one of evaporation, sputtering and CVD methods; as well as Step S4, repeating steps S2 and S3 on the other side of the substrate layer to obtain a flame retardant composite current collector.

Citation Information

Patent Citations

  • Composite current collector, lithium ion battery and vehicle

    CN218677203U

Cited By

  • Composite current collector, pole piece, dual-ion battery and preparation method

    CN120473507A

  • Composite current collector, electrode, dual-ion battery and preparation method

    CN120473507B