Flexible ferroelectric memory device and preparation method thereof

By forming a ferroelectric layer and an organic material channel on a flexible substrate, the production process of flexible ferroelectric memory devices is simplified, the cost is reduced and the performance is improved, and the problem of poor storage performance in the prior art is solved, satisfying the The storage requirements of wearable devices.

CN118900571APending Publication Date: 2024-11-05FUDAN UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974699.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing nonvolatile memory preparation process based on ferroelectric polymers is complicated, resulting in high production costs and poor storage performance, which cannot meet the data processing needs of flexible electronic devices.

Method used

Flexible substrate and atomic layer deposition method are used to dopant hafnium dioxide to form a ferroelectric layer, and organic materials are deposited through vacuum thermal evaporation to form flexible and bendable channels, simplifying the production process and reducing costs.

Benefits of technology

It realizes the preparation of high-performance flexible ferroelectric memory devices, meets the storage needs of wearable devices, and has excellent storage performance and flexibility and bendability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900571A_ABST
    Figure CN118900571A_ABST
Patent Text Reader

Abstract

The invention provides a flexible ferroelectric memory device and a preparation method thereof. The preparation method comprises the following steps: providing a flexible substrate; growing a first metal layer on the substrate to serve as a grid electrode of the memory; doping hafnium oxide on the first metal layer through an atomic layer deposition method to form a ferroelectric layer; growing a second metal layer on the ferroelectric layer to serve as a source electrode and a drain electrode of the memory; an organic material is deposited on the second metal layer through vacuum thermal evaporation to form a flexible bendable channel, the flexible ferroelectric memory device is obtained, the organic material is deposited through vacuum thermal evaporation to form the flexible bendable channel, the production process of the flexible ferroelectric memory device is simplified, the production cost is reduced, and the production efficiency is improved. And the ferroelectric layer is formed by doping hafnium oxide, so that the preparation of the high-performance flexible ferroelectric memory device is realized, and the storage requirement of wearable equipment is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of flexible memory, and in particular to a flexible ferroelectric memory device and a preparation method thereof. Background Art

[0002] Flexible electronics is a technology that makes electronic devices on a flexible plastic substrate to form flexible electronic circuits. Flexible electronics has a wide range of applications due to its unique flexibility and ductility, such as printed radio frequency tags, thin-film solar cells, flexible sensors, flexible electronic displays, etc. Although flexible electronic technologies such as conductive inks and organic light-emitting diodes have matured and are now on the market, flexible memory is a necessary component of flexible circuits, and flexible non-volatile storage technology has not yet been fully broken through, which is still one of the bottlenecks hindering the true commercial application of flexible electronic devices.

[0003] With the rapid advancement of science and technology, the application of artificial intelligence is becoming more and more extensive. Whether it is smart home, autonomous driving or big data processing, it is inseparable from the powerful computing power and data storage behind it. Among them, integrated circuits are the basis of modern electronic devices, and their performance and reliability directly affect the performance of the overall system. Especially in the era of big data and cloud computing, the demand for high-speed, high-capacity flexible non-volatile memory is becoming increasingly urgent.

[0004] In order to solve this problem, people have turned their attention to non-volatile memory based on ferroelectric polymers. However, the preparation process of non-volatile memory based on ferroelectric polymers is not only too complicated, resulting in high production costs, but also the prepared memory has poor storage performance and slow response speed, resulting in the inability of existing memory to meet the data processing needs of flexible electronic devices.

[0005] Therefore, there is an urgent need for a flexible ferroelectric memory device and a preparation method thereof to improve the above problems. Summary of the invention

[0006] The purpose of the present invention is to provide a flexible ferroelectric memory device and a preparation method thereof, which can simplify the production process of the flexible ferroelectric memory device, reduce the production cost, and realize the preparation of a high-performance flexible ferroelectric memory device.

[0007] In a first aspect, the present invention provides a method for preparing a flexible ferroelectric memory device, comprising:

[0008] providing a flexible substrate;

[0009] Growing a first metal layer on the substrate as a gate of the memory;

[0010] doping hafnium dioxide on the first metal layer by atomic layer deposition to form a ferroelectric layer;

[0011] Growing a second metal layer on the ferroelectric layer to serve as a source and a drain of the memory;

[0012] The organic material is deposited on the second metal layer by vacuum thermal evaporation to form a flexible and bendable channel, thereby obtaining a flexible ferroelectric memory device.

[0013] The method of the present invention has the following beneficial effects: providing a flexible substrate; growing a first metal layer on the substrate as a gate of a memory; doping hafnium dioxide on the first metal layer by atomic layer deposition to form a ferroelectric layer; growing a second metal layer on the ferroelectric layer to serve as a source and a drain of the memory; depositing an organic material on the second metal layer by vacuum thermal evaporation to form a flexible and bendable channel, thereby obtaining a flexible ferroelectric memory device. The flexible and bendable channel is formed by depositing organic material by vacuum thermal evaporation, thereby simplifying the production process of the flexible ferroelectric memory device and reducing the production cost. The ferroelectric layer is formed by doping hafnium dioxide, thereby realizing the preparation of a high-performance flexible ferroelectric memory device and meeting the storage requirements of wearable devices.

[0014] Optionally, doping hafnium dioxide on the first metal layer by atomic layer deposition to form a ferroelectric layer includes:

[0015] Aluminum-doped hafnium dioxide is grown by atomic layer deposition to form a mixed layer, and a capping layer is grown on the mixed layer by physical vapor deposition and then rapidly thermally annealed to crystallize the mixed layer to form a ferroelectric layer.

[0016] Optionally, growing aluminum-doped hafnium dioxide by atomic layer deposition to form a mixed layer, and then growing a capping layer on the mixed layer by physical vapor deposition and then rapidly thermally annealing to crystallize the mixed layer to form a ferroelectric layer comprises:

[0017] A mixed layer of aluminum-doped hafnium dioxide was grown by atomic layer deposition to form a 12 nm thick layer, wherein the ratio of aluminum to hafnium was 1:34;

[0018] Then, a titanium nitride capping layer with a thickness of 60 nm is grown on the mixed layer by physical vapor deposition, and then the layer is heated to 550 degrees Celsius and rapidly thermally annealed for 10 seconds to crystallize the mixed layer to form a ferroelectric layer.

[0019] Optionally, depositing an organic material on the second metal layer by vacuum thermal evaporation to form a flexible and bendable channel to obtain a flexible ferroelectric memory device includes:

[0020] The entire device was immersed in a 0.5 mg / L perfluorobutyl mercaptan solution for 20 min to form a monolayer;

[0021] A hard mask alignment mark mask protects the device, and a 50nm thick organic material C8-BTBT is deposited by vacuum thermal evaporation to form a flexible and bendable channel to obtain a flexible ferroelectric memory device, wherein the temperature when depositing the channel is 160 degrees Celsius and the deposition rate is 3nm / min.

[0022] Optionally, growing a first metal layer on the substrate as a gate of the memory includes:

[0023] The flexible substrate is protected by an ultraviolet lithography alignment mark reticle, and a first metal layer is grown by physical vapor deposition as a gate of the memory, wherein the first metal layer is a Ti / W stacked layer.

[0024] Optionally, growing a second metal layer on the ferroelectric layer as a source and a drain of the memory includes:

[0025] The flexible substrate is protected by an ultraviolet lithography alignment mark reticle, and a second metal layer is grown by physical vapor deposition to serve as a source and a drain of the memory, wherein the second metal layer is a W layer.

[0026] Optionally, after the mixed layer is crystallized to form the ferroelectric layer, the method further comprises:

[0027] The titanium nitride capping layer is removed.

[0028] In a second aspect, the present invention further provides a flexible ferroelectric memory device, which is prepared by the method for preparing the flexible ferroelectric memory device in any possible combination of the first aspect above, wherein the flexible ferroelectric memory device comprises a flexible substrate and a gate, a ferroelectric layer doped with hafnium dioxide, a source and a drain, and a flexible and bendable channel composed of organic materials, which are sequentially formed on the flexible substrate from bottom to top.

[0029] The beneficial effect of the flexible ferroelectric memory device of the present invention is that the flexible ferroelectric memory device composed of a ferroelectric layer doped with hafnium dioxide and a flexible and bendable channel composed of organic materials is not only smaller in size but also has a higher storage density, so that the flexible ferroelectric memory device has excellent storage performance while having excellent flexibility and bendability.

[0030] Optionally, the gate is a Ti / W stack, wherein the thickness of the Ti layer is 10 nm, and the thickness of the W layer is 80 nm; the ferroelectric layer includes aluminum and hafnium, and the ratio of aluminum to hafnium is 1:34, and the thickness of the ferroelectric layer is 12 nm.

[0031] Optionally, the source and the drain are W layers; and / or the material of the channel is C8-BTBT with a thickness of 50 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1A schematic flow chart of a method for preparing a flexible ferroelectric memory device provided by an embodiment of the present invention;

[0033] Figure 2 A schematic diagram of the structure of a substrate, an adhesive layer and a photoresist provided in an embodiment of the present invention;

[0034] Figure 3 A schematic structural diagram of a substrate and a first metal layer provided in an embodiment of the present invention;

[0035] Figure 4 A schematic structural diagram of a substrate and a first metal layer after photoresist removal provided by an embodiment of the present invention;

[0036] Figure 5 A schematic diagram of the structure of a mixed layer doped with hafnium dioxide provided in an embodiment of the present invention;

[0037] Figure 6 A schematic diagram of the structure of a mixing layer and a covering layer provided in an embodiment of the present invention;

[0038] Figure 7 A schematic diagram of the structure of a ferroelectric layer after removing the cover layer provided by an embodiment of the present invention;

[0039] Figure 8 A schematic diagram of the structure of a second metal layer, an adhesion layer and a photoresist provided in an embodiment of the present invention;

[0040] Fig. 9 A schematic diagram of the structure of the second metal layer after photoresist removal provided by an embodiment of the present invention;

[0041] Fig.10 A schematic diagram of the structure of a monolayer provided by an embodiment of the present invention;

[0042] Fig.11 A schematic structural diagram of a flexible ferroelectric memory device after depositing an organic material C8-BTBT as a channel provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0044] like Figure 1 As shown, the present invention provides a method for preparing a flexible ferroelectric memory device, comprising:

[0045] S101, providing a flexible substrate. The flexible substrate used in the existing preparation process is limited by high-temperature growth conditions. During preparation, the temperature of the flexible substrate is required to be lower than the melting point of the flexible substrate (about 200°C), and its brittleness is relatively high, which cannot meet the needs of flexible devices. Therefore, MICA (mica) is selected as the flexible substrate to meet the needs of high-temperature processing, so that the prepared flexible ferroelectric memory device can meet the needs of flexible devices.

[0046] S102, growing a first metal layer on the substrate to serve as a gate of the memory.

[0047] In some embodiments, growing a first metal layer on the substrate as a gate of the memory includes: protecting the flexible substrate by an ultraviolet lithography alignment mark reticle, and growing the first metal layer by physical vapor deposition as the gate of the memory, wherein the first metal layer is a Ti / W stack. In some specific embodiments, the thickness of the Ti layer in the Ti / W stack is 10nm, and the thickness of the W layer is 80nm. Ultraviolet lithography, with its high precision and high resolution, can accurately depict the microstructure of the device, while physical vapor deposition can deposit the material layer by layer on the substrate through a physical process in a vacuum environment to form a desired structure. The combination of the two can simply and effectively prepare the stack and improve production efficiency.

[0048] S103, doping hafnium dioxide on the first metal layer by atomic layer deposition to form a ferroelectric layer. It is worth noting that hafnium dioxide, as a material with a high dielectric constant, can change its polarization state under the action of an electric field, thereby realizing information storage. Compared with traditional memory, hafnium dioxide-based ferroelectric memory has higher read and write speeds, lower power consumption and longer data retention time.

[0049] In some embodiments, doping hafnium dioxide on the first metal layer by atomic layer deposition to form a ferroelectric layer includes: growing aluminum-doped hafnium dioxide by atomic layer deposition to form a mixed layer, and then growing a covering layer on the mixed layer by physical vapor deposition and then rapidly thermal annealing to crystallize the mixed layer to form a ferroelectric layer.

[0050] In some specific embodiments, growing aluminum-doped hafnium dioxide by atomic layer deposition to form a mixed layer, then growing a capping layer on the mixed layer by physical vapor deposition and then rapidly thermal annealing to crystallize the mixed layer to form a ferroelectric layer includes: growing aluminum-doped hafnium dioxide (HfO2) by atomic layer deposition to form a 12nm thick mixed layer, wherein the ratio of aluminum to hafnium is 1:34; then growing a 60nm thick titanium nitride (TiN) capping layer on the mixed layer by physical vapor deposition, heating to 550 degrees Celsius and then rapidly thermal annealing for 10S to crystallize the mixed layer to form a ferroelectric layer. The ratio of aluminum to hafnium is 1:34 and combined with heating to 550 degrees Celsius and then rapidly thermal annealing for 10S, all molecular structures of the ferroelectric layer formed after crystallization can be tightly combined, ensuring that the response performance of the flexible ferroelectric memory device finally prepared is significantly improved.

[0051] In some specific embodiments, after the mixed layer is crystallized to form the ferroelectric layer, the method further includes: removing the titanium nitride capping layer. Exemplarily, the titanium nitride capping layer can be removed by wet etching. Specifically, the titanium nitride capping layer can be removed by wet etching with ammonia water: hydrogen peroxide: deionized water = 1:1:5.

[0052] S104, growing a second metal layer on the ferroelectric layer to serve as a source and a drain of the memory.

[0053] In some embodiments, growing a second metal layer on the ferroelectric layer as the source and drain of the memory includes: protecting the flexible substrate by UV lithography alignment mark reticle, and growing the second metal layer by physical vapor deposition as the source and drain of the memory, wherein the second metal layer is a W layer with a thickness of 80nm. Again using UV lithography and physical vapor deposition, the two are combined with each other, which is not only simple to operate and easy to control, but also can accurately depict various parts of the memory, and can also ensure that the prepared flexible ferroelectric memory device has excellent performance and stability by optimizing process parameters and operation procedures.

[0054] S105, depositing an organic material on the second metal layer by vacuum thermal evaporation to form a flexible and bendable channel to obtain a flexible ferroelectric memory device.

[0055] In some embodiments, an organic material is deposited on the second metal layer by vacuum thermal evaporation to form a flexible and bendable channel, and obtaining a flexible ferroelectric memory device includes: immersing the entire device in a 0.5 mg / L perfluorobutyl mercaptan (PFBT) solution for 20 minutes to form a monolayer; a hard mask alignment mark mask protects the device, and vacuum thermal evaporation deposits an organic material C8-BTBT with a thickness of 50 nm to form a flexible and bendable channel to obtain a flexible ferroelectric memory device, wherein, when depositing the channel, the temperature is 160 degrees Celsius and the deposition rate is 3 nm / min.

[0056] The advantages of the embodiments of the present invention are that the preparation method is simple and effective. The laminated structure is manufactured by ultraviolet lithography, physical vapor deposition (PVD), atomic layer deposition, wet etching and high-temperature thermal evaporation, which is easy to manufacture. In addition, a flexible and high-temperature resistant MICA (mica) substrate is selected to provide a basis for device preparation. The use of aluminum-doped hafnium dioxide as a ferroelectric layer can achieve a fast response of the memory. The use of atomic layer deposition technology to grow a dielectric film can accurately control the thickness of the film to obtain a conformal and high-quality dielectric film. The ultraviolet lithography and physical vapor deposition to prepare the memory source, drain and gate are simple to operate.

[0057] For ease of understanding, this embodiment further describes the specific implementation process of the above method in combination with a specific application scenario system. Figure 2-8 As shown, in this embodiment, MICA (mica) is used as a flexible substrate 1, photoresist 2, Ti / W stack is used as a gate 3 (i.e., a first metal layer), aluminum-doped hafnium dioxide is used as a mixed layer 4, titanium nitride (TiN) is used as a cover layer 5, a ferroelectric layer 6, a W layer is used as a source 7 and a drain 8 (i.e., a second metal layer), PFBT is used as a monomolecular layer 9, and an organic material C8-BTBT is used as a channel 10, and specifically includes the following steps:

[0058] Step a, such as Figure 2 As shown, an adhesion layer (not shown) and a photoresist 2 are coated on MICA (mica, i.e., a flexible substrate 1) respectively. The adhesion layer and the photoresist 2 are preferably coated by spin coating (i.e., coating is performed during the rotation of the flexible substrate 1) to improve the uniformity of the adhesion layer and the photoresist 2 coating.

[0059] Step b, such as Figure 3 As shown, a UV lithography alignment mark reticle protects the flexible substrate 1, and a first metal layer (a Ti / W stack of 10 nm Ti and 80 nm W) is grown by physical vapor deposition (PVD) to serve as the gate 3 of the memory.

[0060] Step c, such as Figure 4 As shown, the photoresist 2 is removed.

[0061] Step d, such as Figure 5As shown, aluminum-doped hafnium dioxide (HfO 2 ) is deposited by atomic layer deposition to form a mixed layer 4 with a thickness of 12 nm, wherein the ratio of aluminum to hafnium is 1:34.

[0062] Step e, such as Figure 6 As shown, a 60 nm titanium nitride (TiN) capping layer 5 is grown by physical vapor deposition.

[0063] Step f, such as Figure 6 As shown, rapid thermal annealing is performed at 550 degrees Celsius for 10 seconds to crystallize the mixed layer 4 to form a ferroelectric layer 6.

[0064] Step g, such as Figure 7 As shown, the titanium nitride capping layer 5 is removed by wet etching with a mixture of ammonia water: hydrogen peroxide: deionized water = 1:1:5.

[0065] Step h, such as Figure 8 As shown, an adhesion layer (not shown) and photoresist 2 are applied, a UV lithography alignment mark reticle is used to protect the device, and 80 nmW (ie, the second metal layer) is grown by physical vapor deposition to serve as the source 7 and drain 8 of the memory.

[0066] Step i, such as Fig. 9 As shown, the photoresist 2 is removed.

[0067] Step j, such as Fig.10 As shown, the device was immersed in a 0.5 mg / L perfluorobutyl mercaptan (PFBT) solution for 20 min to form a monolayer 9.

[0068] Step k, such as Fig.11 As shown, a hard mask alignment mark mask protects the device, and C8-BTBT with a thickness of 50 nm is deposited by vacuum thermal evaporation to form a flexible and bendable channel 10 to obtain a flexible ferroelectric memory device, wherein when depositing the channel 10, the temperature is 160 degrees Celsius and the deposition rate is 3nm / min.

[0069] The advantage of the embodiment of the present invention is that the gate of the memory is first defined on the mica substrate by ultraviolet lithography, and Ti / W is grown by physical vapor deposition as the gate electrode. Aluminum-doped hafnium dioxide is grown by atomic layer deposition, and a titanium nitride capping layer is grown by physical vapor deposition, followed by rapid thermal annealing to crystallize the ferroelectric layer. The titanium nitride capping layer is removed by wet etching. The channel of a flexible and bendable ferroelectric memory is realized by vacuum thermal evaporation deposition of C8-BTBT organic semiconductor. The source and drain of a flexible ferroelectric memory device are defined by ultraviolet lithography, and W is grown by physical vapor deposition as the source and drain of the memory. Ti / W and W are grown by ultraviolet lithography and physical vapor deposition as the gate, source and drain of the memory. Aluminum-doped hafnium dioxide is grown by atomic layer deposition as the ferroelectric layer of the memory to realize the storage function. The channel of a flexible and bendable ferroelectric memory is realized by vacuum thermal evaporation deposition of C8-BTBT organic semiconductor.

[0070] like Fig.11 As shown, based on the above-mentioned method for preparing a flexible ferroelectric memory device, the present invention also provides a flexible ferroelectric memory device, which is prepared by the method for preparing a flexible ferroelectric memory device. The flexible ferroelectric memory device includes a flexible substrate 1 and a gate 3, a hafnium dioxide-doped ferroelectric layer 6, a source 7 and a drain 8, and a flexible and bendable channel 10 formed in sequence from bottom to top on the flexible substrate 1. The flexible ferroelectric memory device is not only smaller in size, but also has a higher storage density, so that the flexible ferroelectric memory device has excellent storage performance while having excellent flexibility and bendability.

[0071] like Fig.11 As shown, in some embodiments, the gate 3 is a Ti / W stack, wherein the thickness of the Ti layer is 10 nm, and the thickness of the W layer is 80 nm; the ferroelectric layer 6 includes aluminum and hafnium, and the ratio of aluminum to hafnium is 1:34, and the thickness of the ferroelectric layer 6 is 12 nm; the source 7 and the drain 8 are W layers; the material of the channel 10 is C8-BTBT, and the thickness is 50 nm.

[0072] like Fig.11 As shown, based on the above-mentioned flexible ferroelectric memory device, the present invention also provides a wearable device, including the above-mentioned flexible ferroelectric memory device, wherein the wearable device is one of a smart watch, a smart bracelet, smart glasses, smart headphones, smart clothing, a pedometer and smart shoes, and the flexible ferroelectric memory device based on hafnium dioxide provides strong support for the development of wearable devices. Since wearable devices usually need to be in close contact with the human body, the requirements for their flexibility, lightness and durability are extremely high. Traditional rigid memory devices cannot meet these requirements, while flexible ferroelectric memory devices based on hafnium dioxide can solve this problem well. They not only have excellent storage performance, but also can maintain stable performance in complex environments such as bending and stretching, providing powerful data processing and storage capabilities for wearable devices.

[0073] It should be understood that the above-mentioned flexible ferroelectric memory device of the present invention can be applied to wearable devices as well as terminal devices, and the terminal can be implemented in various forms. For example, the terminal described in the present invention may include mobile terminals such as mobile phones, tablet computers, laptop computers, PDAs, portable media players (PMPs), navigation devices, and fixed terminals such as digital TVs and desktop computers. It will be understood by those skilled in the art that, in addition to components specifically used for mobile purposes, the construction according to the embodiments of the present invention can also be applied to fixed-type terminals.

[0074] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing a flexible ferroelectric memory device, characterized in that: include: providing a flexible substrate; Growing a first metal layer on the substrate as a gate of the memory; doping hafnium dioxide on the first metal layer by atomic layer deposition to form a ferroelectric layer; Growing a second metal layer on the ferroelectric layer to serve as a source and a drain of the memory; The organic material is deposited on the second metal layer by vacuum thermal evaporation to form a flexible and bendable channel, thereby obtaining a flexible ferroelectric memory device.

2. The method according to claim 1, characterized in that Doping hafnium dioxide on the first metal layer by atomic layer deposition to form a ferroelectric layer comprises: Aluminum-doped hafnium dioxide is grown by atomic layer deposition to form a mixed layer, and a capping layer is grown on the mixed layer by physical vapor deposition and then rapidly thermally annealed to crystallize the mixed layer to form a ferroelectric layer.

3. The method according to claim 2, characterized in that Growing aluminum-doped hafnium dioxide by atomic layer deposition to form a mixed layer, then growing a capping layer on the mixed layer by physical vapor deposition and then rapidly thermally annealing to crystallize the mixed layer to form a ferroelectric layer comprises: A mixed layer of aluminum-doped hafnium dioxide was grown by atomic layer deposition to form a 12 nm thick layer, wherein the ratio of aluminum to hafnium was 1:34; Then, a titanium nitride capping layer with a thickness of 60 nm is grown on the mixed layer by physical vapor deposition, and then the layer is heated to 550 degrees Celsius and rapidly thermally annealed for 10 seconds to crystallize the mixed layer to form a ferroelectric layer.

4. The method according to claim 1, characterized in that: Depositing an organic material on the second metal layer by vacuum thermal evaporation to form a flexible and bendable channel, and obtaining a flexible ferroelectric memory device includes: The entire device was immersed in a 0.5 mg / L perfluorobutyl mercaptan solution for 20 min to form a monolayer; A hard mask alignment mark mask protects the device, and a 50nm thick organic material C8-BTBT is deposited by vacuum thermal evaporation to form a flexible and bendable channel to obtain a flexible ferroelectric memory device, wherein the temperature when depositing the channel is 160 degrees Celsius and the deposition rate is 3nm / min.

5. The method according to claim 1, characterized in that: Growing a first metal layer on the substrate as a gate of the memory includes: The flexible substrate is protected by an ultraviolet lithography alignment mark reticle, and a first metal layer is grown by physical vapor deposition as a gate of the memory, wherein the first metal layer is a Ti / W stacked layer.

6. The method according to claim 1, characterized in that Growing a second metal layer on the ferroelectric layer as the source and drain of the memory includes: The flexible substrate is protected by an ultraviolet lithography alignment mark reticle, and a second metal layer is grown by physical vapor deposition to serve as a source and a drain of the memory, wherein the second metal layer is a W layer.

7. The method according to claim 3, characterized in that After the mixed layer is crystallized to form a ferroelectric layer, the method further comprises: The titanium nitride capping layer is removed.

8. A flexible ferroelectric memory device, manufactured by the method for manufacturing a flexible ferroelectric memory device according to any one of claims 1 to 7, characterized in that: The flexible ferroelectric memory device comprises a flexible substrate and a gate electrode, a ferroelectric layer doped with hafnium dioxide, a source electrode and a drain electrode, and a flexible and bendable channel composed of organic materials, which are sequentially formed on the flexible substrate from bottom to top.

9. The flexible ferroelectric memory device according to claim 8, characterized in that: The gate is a Ti / W stack, wherein the thickness of the Ti layer is 10 nm and the thickness of the W layer is 80 nm; and / or the ferroelectric layer comprises aluminum and hafnium, and the ratio of aluminum to hafnium is 1:34, and the thickness of the ferroelectric layer is 12 nm.

10. The flexible ferroelectric memory device according to claim 8, characterized in that: The source and drain are W layers; and / or the material of the channel is C8-BTBT with a thickness of 50 nm.