Flexible Ag2TexSe1-x nanowire film and preparation method thereof
The Ag2TexSe1-x nanowire thermoelectric film prepared by wet chemical synthesis and vacuum suction filtration process solves the problem of low performance of existing flexible thermoelectric materials and realizes high-performance flexible thermoelectric materials, suitable for wearable electronic devices.
Patent Information
- Application Number
- CN202410929006.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
Existing flexible thermoelectric materials and their devices have low performance and are difficult to meet practical application needs, especially in wearable and mobile electronic devices.
Ultrafine Te nanowires were synthesized by wet chemistry, and Ag2TexSe1-x nanowires were prepared by doping Se elements. Combined with vacuum suction filtration process and annealing treatment, flexible Ag2TexSe1-x nanowire thermoelectric films were prepared.
A flexible Ag2TexSe1-x nanowire film with good thermoelectric properties was obtained, which is suitable for the field of flexible wearable electronics, with simple process and low equipment requirements.
Smart Images

Figure CN118900613A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a thermoelectric material, in particular to a flexible Ag2Te x Se 1-x Nanowire film and method for preparing the same. Background Art
[0002] In recent years, the explosive growth of wearable and mobile electronic devices has promoted the research on high-performance, lightweight and flexible forms of power supply. As an energy conversion material, thermoelectric materials can realize the direct conversion between thermal energy and electrical energy. They are expected to convert low-grade thermal energy such as industrial waste heat and automobile exhaust into clean electrical energy. They can also use electrical energy to directly control temperature, which helps to alleviate the damage to the environment caused by refrigerants such as freon. The performance of thermoelectric materials is usually evaluated by the dimensionless thermoelectric figure of merit ZT: ZT = S 2 σT / κ, where σ is electrical conductivity, S is the Seebeck coefficient, κ is thermal conductivity, and T is absolute temperature. The larger the ZT value of the material, the higher the conversion efficiency of thermal energy and electrical energy of the thermoelectric device. However, the performance of flexible thermoelectric materials and their devices is still relatively low, which is difficult to meet the needs of practical applications.
[0003] Nanostructured binary metal chalcogenides are considered to be very promising materials, such as Bi2Te3, PbTe, CdTe, CdSe, Ag2Se, etc. Currently, binary tellurium-based nanowires with smaller diameters can be synthesized by wet chemical methods, which have the advantages of low cost and suitable for large-scale production. Selenium-doped metal telluride ternary alloys have greater tunability in composition, band gap, carrier density and conductivity, and therefore have potential application and research value in the field of thermoelectrics. Summary of the invention
[0004] The purpose of the present invention is to solve the above problems and provide a flexible Ag2Te x Se 1-x NWs film and preparation method thereof, is a ternary silver sulfide compound nanowire film and preparation method thereof, the prepared Ag2Te x Se 1-x NWs flexible thermoelectric film has good thermoelectric performance. This patent first uses a wet chemical method to synthesize ultrafine Te nanowires, and then dopes Se elements to prepare Te x Se 1-x Nanowires, based on which Ag2Te is synthesized x Se 1-x Nanowires, further processed by vacuum filtration and annealing to prepare flexible Ag2Te x Se 1-x Nanowire films.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] The first object of the present invention is to provide a flexible Ag2Te x Se 1-x Nanowire thermoelectric film and preparation method thereof, comprising the following steps:
[0007] S1: Preparation of ultrafine Te NWs; S2: Preparation of Te NWs as precursors x Se 1-x NWs; S3: in Te x Se 1-x Ag source was added to the NWs dispersion to prepare Ag2Te x Se 1-x NWs; S4: Preparation of flexible Ag2Te by vacuum filtration x Se 1-x Thermoelectric thin film material; S5: the thin film is annealed.
[0008] Further, the following steps are included:
[0009] S1: Preparation of ultrafine Te nanowires (Te nanowires are Te NWs): Potassium hydroxide, polyvinyl pyrrolidone and tellurium dioxide are dissolved in ethylene glycol, stirred until completely dissolved, and the mixed solution is heated to 120°C to obtain solution A; hydrazine hydrate is injected into solution A under argon protection, the color of the solution turns black, and the ultrafine Te NWs dispersion is obtained by reaction at 120°C.
[0010] S2:Te x Se 1-x Preparation of NWs: Selenious acid and polyvinyl pyrrolidone are added to ethylene glycol, and stirred at room temperature until completely dissolved to obtain a precursor of Se, which is solution B; ethylene glycol and acetic acid are mixed and stirred to obtain solution C; when the temperature of the ultrafine Te NWs dispersion obtained in step S1 is cooled to 90°C, solution B and solution C are sequentially added dropwise to the ultrafine Te NWs dispersion, and the mixed solution is heated to react to obtain Te x Se 1-x NWs dispersion; Te x Se 1-x The NWs dispersion was naturally cooled to room temperature and centrifuged. The product was washed and redispersed in ethylene glycol, stirred, and ultrasonicated to obtain Te x Se 1-x Ethylene glycol dispersion of NWs.
[0011] S3: Ag2Te x Se 1-xPreparation of NWs dispersion: Dissolve silver nitrate in ethylene glycol to prepare Ag precursor, and add the Ag precursor dropwise into the Te x Se 1-x The NWs were stirred in ethylene glycol dispersion at room temperature, and the product was collected by centrifugation and washed. x Se 1-x NWs were dispersed in anhydrous ethanol and stirred and ultrasonicated to obtain Ag2Te x Se 1-x Dispersion of NWs.
[0012] S4: Ag2Te x Se 1-x Preparation of NWs thin films: Ag2Te x Se 1-x The NWs dispersion was vacuum filtered on a nylon filter membrane to form a film, and then dried to obtain Ag2Te x Se 1-x NWs thin films.
[0013] Furthermore, the preparation method comprises the following steps:
[0014] S1: Preparation of ultrafine Te NWs: Dissolve 15 mmol potassium hydroxide (KOH), 0.5 g polyvinyl pyrrolidone (PVP) and an appropriate amount of tellurium dioxide (TeO2) in 100 mL ethylene glycol (EG) and stir until completely dissolved; heat the mixed solution to 120°C to obtain solution A; under argon protection, quickly inject an appropriate amount of hydrazine hydrate (N2H4·H2O) into solution A, the color of the solution immediately turns black, and react at 120°C for 1 h to obtain ultrafine Te NWs.
[0015] S2:Te x Se 1-x Preparation of NWs: A certain amount of selenious acid (H2SeO3) and 1g PVP were added to 10mL EG and stirred at room temperature until completely dissolved to obtain a Se precursor (solution B); 2.5mL EG and 2mL acetic acid (CH3COOH) were mixed and stirred to obtain a solution C; when the temperature of the Te NWs (step S1) dispersion was cooled to 90°C, solution B and solution C were slowly added dropwise to the Te NWs in sequence; the mixed solution was heated to 110°C for 1h to obtain Te x Se 1-x NWs. Adjust the ratio between Te and Se precursors to obtain Te with different molar Te / Se ratios. x Se 1-x NWs. x Se 1-xThe NWs dispersion was cooled to room temperature and centrifuged. The product was washed alternately with deionized water and ethanol for 3-5 times and redispersed in 100 mL of EG. After stirring for 1 h, it was ultrasonicated for 20 min to obtain Te x Se 1-x EG dispersion of NWs.
[0016] S3: Ag2Te x Se 1-x Preparation of NWs dispersion: A certain amount of silver nitrate (AgNO3) was dissolved in 15 mL EG to obtain Ag precursor; the Ag precursor was added dropwise into Te x Se 1-x The EG dispersion of NWs was stirred at room temperature for 1 h, and the product was collected by centrifugation and washed alternately with deionized water and ethanol for 3-5 times. x Se 1-x NWs were stirred in anhydrous ethanol for 1 h and ultrasonicated for 20 min to obtain Ag2Te x Se 1-x Homogeneous dispersion of NWs.
[0017] S4: Ag2Te x Se 1-x Preparation of NWs thin film: Take Ag2Te x Se 1-x The NWs dispersion was vacuum filtered to form a film on a nylon filter membrane, and then dried under certain conditions to obtain Ag2Te x Se 1-x NWs thin films.
[0018] S5: Ag2Te x Se 1-x The NWs film was annealed at a certain temperature.
[0019] Preferably, in step S1, the appropriate amount of TeO2 is 1.5-3.5 mmol.
[0020] Preferably, in step S1, the appropriate amount of N2H4·H2O is 1 mL.
[0021] Preferably, in step S2, the amount of H2SeO3 is 1.5-3.5 mmol.
[0022] Preferably, in step S3, the amount of AgNO3 is 6-10 mmol.
[0023] Preferably, in step S4, Ag2Te is measured x Se 1-x The volume of NWs dispersion was 100-400 mL.
[0024] Preferably, in step S5, the certain temperature is 220-270°C.
[0025] Preferably, in step S5, the annealing time is 1-3 hours.
[0026] Furthermore, the Ag2Te x Se 1-x NWs refers to Ag2Te x Se 1-x Nanowires.
[0027] The second object of the present invention is to provide a flexible Ag2Te x Se 1-x The nanowire thermoelectric film is prepared by the above preparation method, wherein 0<x<1.
[0028] Preferably, x=0.3, 0.4, 0.5, 0.7.
[0029] Furthermore, the flexible Ag2Te x Se 1-x Nanowire thermoelectric films have good thermoelectric properties and flexibility, and have potential application prospects in the field of flexible wearable electronics.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] This patent first uses a wet chemical method to synthesize Ag2Te x Se 1-x NWs, and then the flexible Ag2Te was prepared by vacuum filtration process. x Se 1-x Nanowire film, and the composition and microstructure of the film were optimized by annealing to obtain flexible Ag2Te x Se 1-x Nanowire thermoelectric film, this technology has simple process and low equipment requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Ag2Te prepared in Example 2 0.4 Se 0.6 Scanning electron microscopy image of nanowires.
[0033] Figure 2 Ag2Te prepared in Example 2 0.4 Se 0.6 Digital photo showing the flexibility of nanowire films. DETAILED DESCRIPTION
[0034] The present invention is described in detail below in conjunction with specific embodiments, but is by no means intended to limit the present invention. Features such as preparation methods, materials, structures or composition ratios not explicitly described in this technical solution are considered to be common technical features disclosed in the prior art.
[0035] The present application provides a flexible Ag2Te x Se 1-x Nanowire thermoelectric film and preparation method thereof, comprising the following five steps: S1: preparation of ultrafine Te NWs; S2: preparation of Te NWs as precursor x Se 1-x NWs; S3: in Te x Se 1-x Ag source was added to the NWs dispersion to prepare Ag2Te x Se 1-x NWs; S4: Preparation of flexible Ag2Te by vacuum filtration x Se 1-x Thermoelectric film; S5: the film is annealed. Compared with the prior art, the flexible thermoelectric material prepared by the present invention has good thermoelectric performance and flexibility, and has potential application prospects in the field of flexible wearable electronics. The technology used has the advantages of simple process and low requirements on equipment.
[0036] The following examples will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several modifications and improvements may be made without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0037] The practice of the present invention may employ conventional techniques of chemistry within the skill of the art. In the following examples, efforts have been made to ensure accuracy with respect to the numbers used (including amounts, temperatures, reaction times, etc.), but some experimental errors and deviations should be taken into account.
[0038] In the following examples, unless otherwise specified, each reagent may be a commercially available product that can be routinely obtained by a person skilled in the art.
[0039] In the following examples, polyvinyl pyrrolidone (PVP) was purchased from Shanghai Titan Technology Co., Ltd., with a molecular weight (MW) of 45,000-58,000.
[0040] Example 1
[0041] This embodiment provides a flexible Ag2Te x Se 1-x NWs thin film and preparation method thereof, in this embodiment, Ag2Te x Se 1-x Ag2Te0.3 Se 0.7 , including the following steps:
[0042] (1) 15 mmol KOH, 0.5 g PVP and 1.5 mmol TeO2 were dissolved in 100 mL EG and stirred until completely dissolved; the mixed solution was heated to 120 °C to obtain solution A; 1 mL N2H4·H2O was quickly injected into solution A under argon protection, and the color of the solution immediately turned black. The reaction was carried out at 120 °C for 1 h to obtain ultrafine Te NWs.
[0043] (2)Te 0.3 Se 0.7 Preparation of NWs: 3.5 mmol of H2SeO3 and 1 g of PVP were added to 10 mL of EG and stirred at room temperature until completely dissolved to prepare a Se precursor (solution B); 2.5 mL of EG and 2 mL of CH3COOH were mixed and stirred to obtain solution C; when the temperature of Te NWs (step 1) was cooled to 90°C, solution B and solution C were slowly added dropwise to Te NWs in sequence; then the mixed solution was heated to 110°C for 1 h to obtain Te 0.3 Se 0.7 NWs. 0.3 Se 0.7 The NWs dispersion was naturally cooled to room temperature and centrifuged. The centrifuged product was washed alternately with deionized water and ethanol for 3-5 times, and the product was redispersed in 100 mL of EG, stirred for 1 h and ultrasonicated for 20 min to obtain Te 0.3 Se 0.7 EG dispersion of NWs;
[0044] (3) Ag2Te 0.3 Se 0.7 Preparation of NWs: 10 mmol of AgNO3 was dissolved in 15 mL of EG to prepare the Ag precursor, which was then added dropwise to the Te 0.3 Se 0.7 The NWs were stirred in EG dispersion at room temperature for 1 h. The product was collected by centrifugation and washed alternately with deionized water and ethanol for 3-5 times. 0.3 Se 0.7 NWs were redispersed in anhydrous ethanol, stirred for 1 h and ultrasonicated for 20 min to obtain Ag2Te 0.3 Se 0.7 Ethanol dispersion of NWs.
[0045] (4) Ag2Te 0.3 Se 0.7 Preparation of NWs film: 60 mg Ag2Te 0.3 Se 0.7The NWs were vacuum filtered onto a nylon filter membrane, and the obtained film was vacuum dried at 60 °C for 12 h to obtain Ag2Te 0.3 Se 0.7 NWs thin films.
[0046] Example 2
[0047] This embodiment provides a flexible Ag2Te x Se 1-x NWs thin film and preparation method thereof, in this embodiment, Ag2Te x Se 1-x Ag2Te 0.4 Se 0.6 , including the following steps:
[0048] (1) 15 mmol KOH, 0.5 g PVP and 2.0 mmol TeO2 powder were dissolved in 100 mL EG and stirred until completely dissolved; the mixed solution was heated to 120°C to obtain solution A; 1 mL N2H4·H2O was quickly injected into solution A under argon protection, and the color of the solution immediately turned black. The reaction was carried out at 120°C for 1 h to obtain ultrafine Te NWs.
[0049] (2)Te 0.4 Se 0.6 Preparation of NWs: 3.0mmol H2SeO3 and 1g PVP were added to 10mL EG and stirred at room temperature until completely dissolved to prepare Se precursor (solution B); 2.5mL EG and 2mL CH3COOH were mixed and stirred to obtain solution C; when the temperature of Te NWs (step 1) was cooled to 90℃, solution B and solution C were slowly added dropwise to Te NWs in sequence; then the mixed solution was heated to 110℃ and kept warm for 1h to obtain Te 0.4 Se 0.6 NWs. 0.4 Se 0.6 The NWs dispersion was naturally cooled to room temperature and centrifuged. The centrifuged product was washed alternately with deionized water and ethanol for 3-5 times. The obtained product was dispersed in 100 mL of EG, stirred for 1 h and ultrasonicated for 20 min to obtain Te 0.4 Se 0.6 EG dispersion of NWs;
[0050] (3) Ag2Te 0.4 Se 0.6 Preparation of NWs: 10 mmol of AgNO3 was dissolved in 15 mL of EG to prepare the Ag precursor, which was then added dropwise to the Te 0.4 Se 0.6The NWs were stirred in EG dispersion at room temperature for 1 h, and the product was collected by centrifugation and washed alternately with deionized water and ethanol for 3-5 times. 0.4 Se 0.6 NWs were dispersed in anhydrous ethanol, stirred for 1 h and ultrasonicated for 20 min to obtain Ag2Te 0.4 Se 0.6 Ethanol dispersion of NWs.
[0051] (4) Ag2Te 0.4 Se 0.6 Preparation of NWs film: Take 60 mg Ag2Te 0.4 Se 0.6 The NWs were vacuum filtered onto a nylon filter membrane, and the obtained film was vacuum dried at 60 °C for 12 h to obtain Ag2Te 0.4 Se 0.6 NWs thin films.
[0052] (5) Ag2Te 0.4 Se 0.6 Treatment of NWs films: Ag2Te 0.4 Se 0.6 The NWs film was annealed at 270 °C for 2 h to obtain Ag2Te 0.4 Se 0.6 NWs thin films.
[0053] like Figure 1 The preparation of Ag2Te in Example 2 is shown 0.4 Se 0.6 SEM images of NWs show that the synthesized Ag2Te 0.4 Se 0.6 It is a one-dimensional nanowire, and the diameter of the nanowire is relatively uniform.
[0054] Figure 2 Ag2Te of Example 2 0.4 Se 0.6 Digital photo showing the flexibility of NWs films. The Ag2Te 0.4 Se 0.6 The nanowire film was able to bend well, indicating that it has good flexibility.
[0055] Example 3
[0056] This embodiment provides a flexible Ag2Te x Se 1-x NWs thin film and preparation method thereof, in this embodiment, Ag2Te x Se 1-x Ag2Te 0.5 Se 0.5 , including the following steps:
[0057] (1) 15 mmol KOH, 0.5 g PVP and 1.5 mmol TeO2 were dissolved in 100 mL EG and stirred until completely dissolved; the mixed solution was heated to 120 °C to obtain solution A; 1 mL N2H4·H2O was quickly injected into solution A under argon protection, and the color of the solution immediately turned black. The reaction was carried out at 120 °C for 1 h to obtain ultrafine Te NWs.
[0058] (2)Te 0.5 Se 0.5 Preparation of NWs: 1.5 mmol H2SeO3 and 1 g PVP were added to 10 mL EG and stirred at room temperature until completely dissolved to prepare Se precursor (solution B); 2.5 mL EG and 2 mL CH3COOH were mixed and stirred to obtain solution C; when the temperature of Te NWs (step 1) was cooled to 90°C, solution B and solution C were slowly added dropwise to Te NWs in sequence; then the mixed solution was heated to 110°C and kept warm for 1 h to obtain Te 0.5 Se 0.5 NWs. 0.5 Se 0.5 The NWs dispersion was naturally cooled to room temperature and centrifuged. The centrifuged product was washed alternately with deionized water and ethanol for 3-5 times, and the obtained product was redispersed in 100 mL of EG, stirred for 1 h and ultrasonicated for 20 min to obtain Te 0.5 Se 0.5 EG dispersion of NWs;
[0059] (3) Ag2Te 0.5 Se 0.5 Preparation of NWs: 6 mmol of AgNO3 was dissolved in 15 mL of EG to prepare the Ag precursor, which was then added dropwise to the Ag2Te 0.5 Se 0.5 The NWs were stirred in EG dispersion at room temperature for 1 h, the product was collected by centrifugation, and washed alternately with deionized water and ethanol for 3-5 times. 0.5 Se 0.5 NWs were dispersed in anhydrous ethanol, stirred for 1 h and ultrasonicated for 20 min to obtain Ag2Te 0.5 Se 0.5 Ethanol dispersion of NWs.
[0060] (4) Ag2Te 0.5 Se 0.5 Preparation of NWs film: Take 60 mg Ag2Te 0.5 Se 0.5The NWs were vacuum filtered onto a nylon filter membrane, and the obtained film was vacuum dried at 60 °C for 12 h to obtain Ag2Te 0.5 Se 0.5 NWs thin films.
[0061] Example 4
[0062] This embodiment provides a flexible Ag2Te x Se 1-x NWs thin film and preparation method thereof, in this embodiment, Ag2Te x Se 1-x Ag2Te 0.7 Se 0.3 , including the following steps:
[0063] (1) 15 mmol KOH, 0.5 g PVP and 3.5 mmol TeO2 were dissolved in 100 mL EG and stirred until completely dissolved; the mixed solution was heated to 120°C to obtain solution A; 1 mL N2H4·H2O was quickly injected into solution A under argon protection, and the color of the solution immediately turned black. The solution was reacted at 120°C for 1 h to obtain ultrafine Te NWs.
[0064] (2)Te 0.7 Se 0.3 Preparation of NWs: 1.5 mmol H2SeO3 and 1 g PVP were added to 10 mL EG and stirred at room temperature until completely dissolved to prepare Se precursor (solution B); 2.5 mL EG and 2 Ml CH3COOH) were mixed and stirred to obtain solution C; when the temperature of Te NWs (step 1) was cooled to 90°C, solution B and solution C were slowly added dropwise to Te NWs in sequence; then the mixed solution was heated to 110°C and kept warm for 1 h to obtain Te 0.7 Se 0.3 NWs. 0.7 Se 0.3 The NWs dispersion was naturally cooled to room temperature and centrifuged. The centrifuged product was washed alternately with deionized water and ethanol for 3-5 times. The obtained product was dispersed in 100 mL of EG, stirred for 1 h and ultrasonicated for 20 min to obtain Te 0.7 Se 0.3 EG dispersion of NWs;
[0065] (3) Ag2Te 0.7 Se 0.3 Preparation of NWs: 10 mmol of AgNO3 was dissolved in 15 mL of EG to prepare the Ag precursor, which was then added dropwise to the Ag2Te 0.7 Se 0.3The NWs were stirred in EG dispersion at room temperature for 1 h, the product was collected by centrifugation, and washed alternately with deionized water and ethanol for 3-5 times. 0.7 Se 0.3 NWs were dispersed in anhydrous ethanol, stirred for 1 h and ultrasonicated for 20 min to obtain Ag2Te 0.7 Se 0.3 Ethanol dispersion of NWs.
[0066] (4) Ag2Te 0.7 Se 0.3 Preparation of NWs film: 60 mg Ag2Te 0.7 Se 0.3 The NWs were vacuum filtered onto a nylon filter membrane, and the obtained film was vacuum dried at 60 °C for 12 h to obtain Ag2Te 0.7 Se 0.3 NWs thin film (Ag2Te 0.7 Se 0.3 Nanowire thermoelectric film).
[0067] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A flexible Ag2Te x Se 1-x Nanowire film and preparation method thereof, characterized in that: It includes the following five steps: S1: Preparation of ultrafine Te nanowires: Potassium hydroxide, polyvinyl pyrrolidone and tellurium dioxide were dissolved in ethylene glycol, stirred until completely dissolved, and the mixed solution was heated to 120°C to obtain solution A; hydrazine hydrate was injected into solution A under argon protection, and the color of the solution turned black. Ultrafine Te NWs dispersion was obtained by reaction at 120°C; S2:Te x Se 1-x Preparation of NWs: Selenious acid and polyvinyl pyrrolidone are added to ethylene glycol, and stirred at room temperature until completely dissolved to prepare a Se precursor, which is solution B; ethylene glycol and acetic acid are mixed and stirred to obtain solution C; when the temperature of the ultrafine Te NWs dispersion obtained in step S1 is cooled to 90°C, solution B and solution C are sequentially added dropwise to the ultrafine Te NWs dispersion, and the mixed solution is heated to react to obtain Te x Se 1-x NWs dispersion; Te x Se 1-x The NWs dispersion was naturally cooled to room temperature and centrifuged. The product was washed and redispersed in ethylene glycol, stirred, and ultrasonicated to obtain Te x Se 1-x Ethylene glycol dispersion of NWs; S3: Ag2Te x Se 1-x Preparation of NWs dispersion: Dissolve silver nitrate in ethylene glycol to prepare Ag precursor, and add the Ag precursor dropwise into the Te x Se 1-x The NWs were stirred in ethylene glycol dispersion at room temperature, and the product was collected by centrifugation and washed. x Se 1-x NWs were dispersed in anhydrous ethanol and stirred and ultrasonicated to obtain Ag2Te x Se 1-x dispersion of NWs; S4: Ag2Te x Se 1-x Preparation of NWs thin films: Ag2Te x Se 1-x The NWs dispersion was vacuum filtered on a nylon filter membrane to form a film, and then dried to obtain Ag2Te x Se 1-x NWs thin film; S5: Ag2Te x Se 1-x Annealing of NWs film to obtain flexible Ag2Te x Se 1-x NWs thermoelectric thin films.
2. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: It includes the following five steps: S1: Preparation of ultrafine Te NWs: 15 mmol potassium hydroxide, 0.5 g polyvinyl pyrrolidone and tellurium dioxide were dissolved in 100 mL ethylene glycol, stirred until completely dissolved, and the mixed solution was heated to 120 °C to obtain solution A; hydrazine hydrate was quickly injected into solution A under argon protection, and the color of the solution immediately turned black. The solution was reacted at 120 °C for 1 h to obtain ultrafine Te NWs; S2:Te x Se 1-x Preparation of NWs: A certain amount of selenious acid and 1 g of polyvinyl pyrrolidone were added to 10 mL of ethylene glycol and stirred at room temperature until completely dissolved to obtain a Se precursor, which is solution B; 2.5 mL of ethylene glycol and 2 mL of acetic acid were mixed and stirred to obtain solution C; when the temperature of the ultrafine Te NWs dispersion obtained in step S1 was cooled to 90°C, solution B and solution C were sequentially added dropwise to the Te NWs dispersion; the mixed solution was heated to 110°C for reaction for 1 h to obtain Te x Se 1-x NWs, Te x Se 1-x The NWs dispersion was cooled to room temperature and centrifuged. The product was washed alternately with deionized water and ethanol for 3-5 times and dispersed in 100 mL of ethylene glycol. After stirring for 1 h, it was ultrasonicated for 20 min to obtain Te x Se 1-x EG dispersion of NWs; S3: Ag2Te x Se 1-x Preparation of NWs dispersion: Silver nitrate was dissolved in 15 mL of ethylene glycol to obtain Ag precursor; the Ag precursor was added dropwise to the Te x Se 1-x The NWs were stirred in ethylene glycol dispersion at room temperature for 1 h, and the product was collected by centrifugation and washed alternately with deionized water and ethanol for 3-5 times. x Se 1-x NWs were stirred in anhydrous ethanol for 1 h and ultrasonicated for 20 min to obtain Ag2Te x Se 1-x NWs dispersion; S4: Ag2Te x Se 1-x Preparation of NWs thin film: Take Ag2Te x Se 1-x The NWs dispersion was vacuum filtered on a nylon filter membrane to form a film, and then dried to obtain Ag2Te x Se 1-x NWs thin film; S5: Ag2Te x Se 1-x Annealing of NWs film to obtain flexible Ag2Te x Se 1-x Nanowire thermoelectric films.
3. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: In step S1, the amount of tellurium dioxide is 1.5-3.5 mmol.
4. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: In step S1, the amount of hydrazine hydrate is 1 mL.
5. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: In step S2, the amount of selenious acid is 1.5-3.5 mmol.
6. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: In step S3, the amount of silver nitrate is 6-10 mmol.
7. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: In step S4, the drying condition is vacuum drying at 60° C. for 12 hours.
8. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: In step S5, the annealing temperature is 220-270°C.
9. A flexible Ag2Te according to claim 1 x Se 1-x Nanowire film and preparation method thereof, characterized in that: In step S5, the annealing time is 1-3 hours.
10. A flexible Ag2Te obtained by the preparation method according to any one of claims 1 to 9 x Se 1-x A nanowire film, characterized in that The range of x is 0<x<1.