Preparation method and application of carbon nanotube-sodium-philic metal cathode-free sodium metal battery electrode material
Through the preparation of carbon nanotube-sodium-philic metal anode-free sodium metal battery electrode materials, the problems of low energy density and short cycle life of sodium metal batteries are solved, and the battery performance with high energy density and long cycle life is achieved, with excellent chemistry and air stability.
Patent Information
- Application Number
- CN202480001132.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-10
AI Technical Summary
The existing sodium metal batteries have low energy density and short cycle life. The negative-electrode sodium metal batteries have irreversible loss of active sodium and unstable solid electrolyte interface phase problems, which hinder their development.
Using carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material preparation method, modify carbon nanotubes and sodium-philic metal salts through dielectric barrier plasma equipment to form porous three-dimensional structural electrode material, and improve sodium ion deposition and dissolution Conductivity and ion transfer rate enhance the cycling stability of the battery.
It achieves excellent structural stability and conductivity of the electrode material, extends the cycle life of sodium metal batteries, improves energy density, and has excellent chemical stability and air stability, improving safety.
Smart Images

Figure CN118900822A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium metal batteries, and in particular to a method for preparing a carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material and an application thereof. Background Art
[0002] In the era of low-carbon energy, electrification of transportation and intelligent equipment, the development of renewable energy not only provides a safe guarantee for the sustainable development of human energy, but also can alleviate problems such as climate warming and environmental pollution. Metallic sodium is considered to be the most likely negative electrode material to replace metallic lithium due to its high theoretical capacity, abundant reserves and low cost. However, the energy density of sodium-ion batteries is usually less than 150Wh kg -1 , which is only half of that of lithium-ion batteries of the same system. Using sodium as a metal anode is the most promising way to increase the energy density of sodium-ion batteries because it has a high theoretical capacity (1166 mAh g –1 ) and a low redox potential (–2.71 V vs standard hydrogen electrode).
[0003] However, sodium metal is highly active, soft and sticky, which makes it difficult to process ultra-thin metal sodium negative electrodes. Currently, excessive ultra-thick metal sodium is often used as the negative electrode, which greatly reduces the actual energy density of the battery. "Anode-free" sodium metal battery (AFSMB) has the advantages of high energy density, low cost, and high safety. It is one of the most promising next-generation high-energy density battery systems. However, the sodium source only comes from the positive electrode material. The irreversible loss of active sodium, unstable solid electrolyte interface phase, and short cycle life have seriously hindered its development. Summary of the invention
[0004] In view of the deficiencies in the prior art, one of the purposes of the present invention is to solve one or more problems in the prior art. For example, one of the purposes of the present invention is to provide a negative electrode-free sodium metal battery electrode material with long cycle life and high energy density.
[0005] In one aspect, the present invention provides a method for preparing a carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material, comprising the following steps:
[0006] Step 1, modifying the carbon nanotubes by using a dielectric barrier plasma device;
[0007] Step 2, mixing and stirring the modified carbon nanotubes with a sodium-philic metal salt to obtain a precursor slurry;
[0008] Step three, drying the precursor slurry, placing it in a tubular furnace after drying, and introducing a reducing gas to heat the reaction to obtain a carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material.
[0009] Furthermore, the carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material is a porous three-dimensional structure, and the porous three-dimensional structure includes a skeleton formed by the interweaving of the carbon nanotubes and the sodium-philic metal salt uniformly attached to the skeleton.
[0010] Furthermore, in step one, the modification treatment of the carbon nanotubes includes placing the carbon nanotubes in a dielectric barrier plasma discharge equipment mold and introducing an inert gas for activation treatment; the inert gas is one or more combinations of argon, nitrogen, and argon-hydrogen mixed gas.
[0011] Furthermore, in step 2, magnetic stirring is used to obtain the precursor slurry; the rotation speed of the magnetic stirring is 100r / min~300r / min, and the stirring time is 1h~5h; in step 3, the drying treatment is vacuum drying, the vacuum drying time is 10h~24h, and the drying temperature is 40℃~80℃.
[0012] Furthermore, in step three, the heating temperature of the heating reaction is increased to 200°C to 500°C at a heating rate of 1°C / min to 10°C / min, and then maintained at 200°C to 500°C for 30min to 5h until the reaction is completed.
[0013] Furthermore, the sodium-philic metal salt is one or more combinations of ferric chloride, tin chloride, silver nitrate, magnesium acetate, etc.; the mass ratio of the sodium-philic metal salt to the carbon nanotube is (0-10):1.
[0014] In a second aspect, the present invention further provides a carbon nanotube-sodium-philic metal anode-free sodium metal battery electrode material, wherein the carbon nanotube-sodium-philic metal anode-free sodium metal battery electrode material is prepared by the carbon nanotube-sodium-philic metal anode-free sodium metal battery electrode material preparation method as described above.
[0015] In a third aspect, the present invention further provides a method for preparing a composite electrode sheet for a negative electrode-free sodium metal battery, comprising the following steps:
[0016] The carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material is mixed with a binder and a solvent to obtain a slurry; the slurry is coated on a negative electrode current collector and dried to obtain a composite electrode sheet; the carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material is prepared by the carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material preparation method as described above, or the carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material as described above.
[0017] Furthermore, the coating thickness of the slurry on the negative electrode current collector is 0.001 mm to 0.05 mm.
[0018] In a fourth aspect, the present invention further provides a composite sodium metal battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode is a composite electrode sheet prepared by the method for preparing a composite electrode sheet for a negative electrode-free sodium metal battery as described above.
[0019] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:
[0020] (1) The electrode material prepared by the method of the present invention has a stable structure and excellent conductive properties, and can be applied to electrode materials for negative electrode-free sodium metal batteries. The entire preparation process is controllable, the synthesis cycle is short, and the operation is simple.
[0021] (2) After the metal salt used in the present invention is reduced to metal, the Fe atomic metal has an affinity for sodium ions, inducing the deposition and dissolution of sodium during the battery charge and discharge process, thereby improving the conductivity and ion transfer rate of the electrode, thereby improving the cycle stability and service life of the battery.
[0022] (3) The electrode material of the present invention has good chemical stability and electrochemical performance, excellent air stability, and high safety.
[0023] (4) The electrode material of the present invention uses MWCNT (multi-walled carbon nanotube) as a conductive network, has a high specific surface area, can make the electric field distribution uniform, delay dendrite growth, and has a light weight, which can improve the energy density of the sodium metal battery and extend its cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and other objects and features of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:
[0025] Figure 1 The present invention is a flow chart of a method for preparing a carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material.
[0026] Figure 2 This is the X-ray diffraction pattern (XRD) of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material obtained in Example 1 of the present invention.
[0027] Figure 3 This is a voltage distribution diagram of the (Na / diaphragm / negative electrode) constant current sodium electroplating of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material obtained in Example 1 of the present invention.
[0028] Figure 4 This is the first charge and discharge curve of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material (sodium vanadium phosphate / diaphragm / negative electrode) obtained in Example 1 of the present invention.
[0029] Figure 5This is a half-cell (Na / diaphragm / negative electrode) cycle diagram of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material obtained in Example 2 of the present invention.
[0030] Figure 6 It is a cycle diagram of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material half-cell (NVP / diaphragm / negative electrode) obtained in Example 3 of the present invention.
[0031] Figure 7 It is a rate diagram of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material half-cell (NVP / diaphragm / negative electrode) obtained in Example 4 of the present invention.
[0032] Figure 8 This is the electrochemical impedance spectrum (EIS) of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material obtained in Example 5 of the present invention.
[0033] Fig. 9 This is a voltage distribution diagram of the (Na / diaphragm / negative electrode) constant current sodium electroplating of the carbon nanotube negative electrode-free sodium metal battery electrode material obtained in Comparative Example 1 of the present invention.
[0034] Fig.10 This is a (NVP / diaphragm / negative electrode) cycle diagram of the carbon nanotube-iron negative electrode-free sodium metal battery electrode material obtained in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with specific examples and drawings. In the following examples, if no special description is given to the experimental methods, all are conventional operations, and the reagents used are commercially available.
[0036] Hereinafter, a carbon nanotube-sodium-philic metal electrode material and a preparation method thereof according to the present invention will be described in detail with reference to the accompanying drawings and exemplary embodiments.
[0037] One aspect of the present invention provides a method for preparing a carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material, such as Figure 1 As shown, the specific steps include:
[0038] S1, modifying the carbon nanotubes through a dielectric barrier plasma device;
[0039] S2, mixing and stirring the modified carbon nanotubes with a sodium-philic metal salt to obtain a precursor slurry; specifically, mixing and stirring the modified carbon nanotubes, the sodium-philic metal salt and a solvent to obtain a precursor slurry;
[0040] S3, drying the precursor slurry, placing it in a tubular furnace after drying, and introducing a reducing gas to heat the reaction to obtain a carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material.
[0041] In some embodiments, the carbon nanotubes (CNTs) are modified by a dielectric barrier plasma device to provide nucleation sites for sodium-philic metal salts. After the modified carbon nanotubes are mixed with sodium-philic metal salts, the modification can provide active sites for reducing metal nucleation, allowing the metal to better composite with CNT, enhancing the affinity of the electrode material for sodium ions, and improving the electrochemical performance of the negative electrode-free sodium metal battery. In some embodiments, the carbon nanotubes can be modified by an argon dielectric barrier plasma. For example, the plasma device power can be 100W to 400W, and the treatment time can be 1min to 30min; that is, the plasma device power can be 100W, 150W, 200W, 250W, 300W, 350W, 400W, and the treatment time can be 1min, 2min, 5min, 8min, 10min, 15min, 20min, 25min, 30min, as long as it is within the aforementioned range. Preferably, the plasma device power can be 300W and the treatment time can be 5min.
[0042] In some embodiments, the sodium affinity of the metal can be used to effectively induce uniform deposition of sodium ions after being combined with carbon nanotubes as a conductive network, thereby improving the energy density of the sodium metal battery and extending the cycle life of the sodium metal battery.
[0043] In some embodiments, the mass ratio of the sodium-philic metal salt and the CNT can be (0-10) g:1 g. The value of the sodium-philic metal salt in the above mass ratio can be 0, or it can be 0.2, 0.5, 0.8, 1, 1.5, 2, 3, 5, 7, 9, 10, as long as it is within the aforementioned range. For example, the mass ratio of the sodium-philic metal salt and the CNT can be (0-9):1, (2-7):1, (4-6):1 or a combination of the above ranges. Preferably, the mass ratio of the sodium-philic metal salt and the CNT can be 3:1. Under the above preferred ratios, the sodium-philic metal is more evenly distributed, the porosity is high, the specific surface area is large, dealloying is easier, and it is more conducive to uniform deposition of sodium metal.
[0044] In some embodiments, the sodium-philic metal salt can be one or more combinations of ferric chloride, tin chloride, silver nitrate, magnesium acetate, and the like.
[0045] In some embodiments, the above binder may be polyvinylidene fluoride, polyacrylic acid or polytetrafluoroethylene.
[0046] In some embodiments, the porous three-dimensional structure composed of interwoven carbon nanotubes is formed by uniformly attaching sodium-affinity metals to the walls of carbon nanotubes. The interwoven carbon nanotubes serve as the basic skeleton of the electrode material and play the role of a supporting network. In addition to stabilizing the structure of the electrode material, they can also reduce the local current density of the material. The sodium-affinity metal is attached to the wall of the carbon nanotubes. The carbon nanotubes are composited with the sodium-affinity metal to construct an electrode material in which sodium ions can be uniformly deposited, which delays the formation of dendrites, improves the cycle life of the battery, and effectively alleviates the problem of low coulomb efficiency of the negative electrode-free sodium metal battery during cycling. The prepared material has high stability and high electrochemical performance. Carbon nanotubes have the characteristics of uniform current density distribution, uniform temperature field distribution, and uniform stress field distribution, which is more conducive to the negative electrode-free sodium metal battery system.
[0047] In some embodiments, the carbon nanotubes may be multi-walled carbon nanotubes, which can effectively conduct electrons, and the interlayer gaps of the multi-walled carbon nanotubes can achieve rapid sodium ion transport, which can improve the reaction kinetics of the electrode material during cycling.
[0048] In some embodiments, introducing a reducing gas into the precursor material and heating it until the reaction is completed can include placing the precursor material in a vacuum tube furnace, heating the temperature to 200°C to 500°C at a heating rate of 1°C / min to 10°C / min, and then keeping it at 200°C to 500°C for 30min to 2h until the reaction is completed; that is, the heating rate can be 1°C / min, 2°C / min, 4°C / min, 5°C / min, 8°C / min, 10°C / min; the temperature can be increased to 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, the insulation temperature can be 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, and the insulation time can be 30min, 35min, 40min, 50min, 55min, 1h, 1.5h, 2h; as long as it is within the aforementioned range. For example, the temperature can be raised to 220°C to 350°C at a heating rate of 3°C / min to 7°C / min in a tubular furnace, and then kept at 220°C to 350°C for 30min to 60min until the reaction is completed. For another example, the temperature can be raised to 280°C to 440°C at a heating rate of 4°C / min to 6°C / min in a tubular furnace, and then kept at 280°C to 440°C for 1h to 2h until the reaction is completed.
[0049] In some embodiments, the modified carbon nanotubes, the sodium-philic metal salt and the solvent are mixed and magnetically stirred to obtain a precursor solution. The speed of the magnetic stirring can be 100 r / min to 300 r / min. For example, the speed of the magnetic stirring can be 150 r / min, and the stirring time can be 5 hours.
[0050] In some embodiments, the drying may be vacuum drying. The vacuum drying time may be 8 hours to 24 hours, and the drying temperature may be 40° C. to 80° C. For example, the vacuum drying time may be 10 hours to 15 hours, and the drying temperature may be 50° C. to 70° C.
[0051] Another aspect of the present invention provides a carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material, which is a composite material formed by a porous three-dimensional structure composed of interwoven carbon nanotubes as a skeleton and sodium-philic metals uniformly attached to the walls of carbon nanotubes, wherein CNTs are modified by a dielectric barrier plasma device. The interwoven carbon nanotubes serve as the basic skeleton of the electrode material and play the role of a supporting network. In addition to stabilizing the structure of the electrode material, they can also reduce the local current density of the material. The carbon nanotubes have the characteristics of uniform current density distribution, uniform temperature field distribution, and uniform stress field distribution, which is more conducive to the negative electrode-free sodium metal battery system. The sodium-philic metal is attached to the wall of the carbon nanotube, and the carbon nanotubes are composited with the sodium-philic metal to construct an electrode material in which sodium ions can be uniformly deposited, which delays the formation of dendrites, improves the cycle life of the battery, and effectively alleviates the problem of low coulomb efficiency of the negative electrode-free sodium metal battery during circulation. The prepared material has high stability and high electrochemical performance.
[0052] Another aspect of the present invention provides a method for preparing a composite electrode sheet for a negative electrode-free sodium metal battery, which may include the following steps:
[0053] The carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material is mixed with an adhesive and a solvent to obtain a slurry; the slurry is coated on a negative electrode current collector and dried to obtain a composite electrode sheet.
[0054] In some embodiments, the binder may be polyvinylidene fluoride, polyacrylic acid or polytetrafluoroethylene, etc. The mass ratio of the carbon nanotube-sodium-affinity metal-free negative electrode sodium metal battery electrode material to the binder may be adjusted according to the actual battery setting requirements. For example, the mass ratio of the carbon nanotube-sodium-affinity metal-free negative electrode sodium metal battery electrode material to the conductive agent may be 9:1, 7:3 or 9.5:0.5. After the carbon nanotube-sodium-affinity metal-free negative electrode sodium metal battery electrode material is mixed with the binder, it may be ground to obtain a mixture. For example, the grinding time may be 20 min to 30 min.
[0055] In some embodiments, the negative electrode current collector may be an existing negative electrode current collector such as aluminum foil, copper foil, zinc foil, or iron foil.
[0056] In some embodiments, the slurry coating thickness on the negative electrode current collector can be 0.001mm to 0.05mm; specifically, the slurry coating thickness can be 0.001mm, 0.002mm, 0.005mm, 0.008mm, 0.01mm, 0.015mm, 0.02mm, 0.025mm, 0.03mm, 0.035mm, 0.04mm, 0.045mm, 0.05mm, as long as it is within the aforementioned range. For example, the coating thickness can be 0.009mm to 0.045mm, 0.007mm to 0.012mm, 0.01mm to 0.018mm or a combination of the above ranges.
[0057] Another aspect of the present invention provides a composite negative electrode-free sodium metal battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode is a composite electrode sheet prepared by the above-mentioned method for preparing a composite electrode sheet for a negative electrode-free sodium metal battery, wherein the positive electrode and the negative electrode are located on both sides of the separator, and the positive electrode can be a sodium metal sheet. The diameter of the sodium metal sheet can be 16 mm and the thickness can be 0.1 mm to 0.5 mm. Of course, the diameter and thickness of the positive electrode material of the present invention are not limited thereto and can be adjusted according to the actual needs of the battery.
[0058] In some embodiments, the electrolyte may be a sodium hexafluorophosphide / sodium tetrafluoroborate / diethylene glycol dimethyl ether solution. The separator may be a polypropylene film. Of course, it should be understood that the electrolyte and separator of the composite sodium metal battery of the present invention are not limited thereto.
[0059] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific examples, but the content of the present invention is not limited to the following examples.
[0060] Example 1
[0061] Step 1, placing MWCNT (multi-walled carbon nanotube) powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0062] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 3:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0063] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0064] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride in a mass ratio of 8:2, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0065] The X-ray diffraction (XRD) pattern of the composite electrode material obtained in this example is as follows: Figure 2 As shown, the XRD diffraction peaks correspond to the characteristic peaks, and after complexing with the sodium-philic metal Fe, only the diffraction peaks are superimposed without the appearance of impurity peaks. Figure 3 This is a voltage distribution diagram of constant current sodium electroplating (Na / diaphragm / negative electrode) of the carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material obtained in Example 1 of the present invention. It can be seen from the figure that the electrode material has a low nucleation overpotential, and sodium is easily deposited on the surface of the electrode sheet after the surface is composited with the sodium-philic metal. Figure 4 This is the first charge and discharge curve of the composite electrode material battery (NVP / diaphragm / negative electrode) obtained in this example. It can be seen from the figure that the first discharge capacity is as high as 87.9 mAh g -1 .
[0066] Example 2
[0067] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0068] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 4:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0069] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0070] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0071] The battery assembled with the composite electrode material obtained in this example has a voltage range of 0V to 3V and a current of 3mA cm -2 The cycling performance at current density is Figure 5 As shown, the -2 SEI was generated after 5 cycles at low current density, and the coulombic efficiency was close to 100% after 250 h of cycling.
[0072] Example 3
[0073] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0074] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 5:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0075] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0076] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0077] The battery assembled with the composite electrode material obtained in this example has a voltage range of 2.5V to 3.8V and a current density of 117.6mAh g -1 The cycling performance at current density is Figure 6 As shown, the first discharge capacity is 85.4 mAh g -1 After 120 cycles, the Coulomb efficiency reached 95.4%.
[0078] Example 4
[0079] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0080] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 6:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0081] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0082] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0083] The battery assembled with the composite electrode material obtained in this example has a cycle performance of 0V to 2.5V at different current densities. Figure 7 As shown, the current density reaches 352.8 mAh g -1The Coulomb efficiency is still higher than 90%.
[0084] Example 5
[0085] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0086] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 7:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0087] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0088] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0089] The battery assembled with the composite electrode material obtained in this example was subjected to an AC impedance test. Figure 8 As shown, it can be seen that there is low impedance between the electrolyte material and the electrode material, indicating that the composite electrode material has excellent interfacial dynamics.
[0090] Example 6
[0091] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0092] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 8:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0093] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0094] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0095] The battery assembled with the composite electrode material obtained in this embodiment has stable electrochemical performance and long cycle life within the voltage range of 2.5V to 3.8V.
[0096] Example 7
[0097] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0098] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 9:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0099] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0100] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0101] The battery assembled with the composite electrode material obtained in this embodiment has stable electrochemical performance and long cycle life within the voltage range of 2.5V to 3.8V.
[0102] Example 8
[0103] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 150V / 200V, the current to 2A / 1.5A, ensuring that the treatment is carried out at a power of 300 watts for 5 minutes, and obtaining the treated MWCNT.
[0104] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 10:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0105] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0106] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0107] The battery assembled with the composite electrode material obtained in this embodiment has stable electrochemical performance and long cycle life within the voltage range of 2.5V to 3.8V.
[0108] Example 9
[0109] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 100V and the current to 2A, ensuring that the treatment is carried out at a power of 200 watts for 5 minutes, and obtaining the treated MWCNT.
[0110] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 3:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0111] Step 3, place the precursor slurry in a vacuum drying oven at 80°C and dry it for 8 hours. After drying, place it in a tubular furnace and heat it to 350°C at a heating rate of 5°C / min, then keep it warm for 3 hours, introduce reducing gas and heat until the reaction is completed, cool it to room temperature in the tubular furnace, and then take out the powder to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0112] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0113] The battery assembled with the composite electrode material obtained in this embodiment has stable electrochemical performance and long cycle life within the voltage range of 2.5V to 3.8V.
[0114] Example 10
[0115] Step 1, placing MWCNT powder in a dielectric barrier plasma mold, introducing nitrogen gas, adjusting the voltage to 70V and the current to 4A, ensuring that the treatment is carried out at a power of 280 watts for 5 minutes to obtain treated MWCNT.
[0116] Step 2, add sodium-philic metal salt FeCl3 and MWCNT in a mass ratio of 3:1 into a beaker, add 10 ml of N-methylpyrrolidone, and place it on a magnetic stirrer and stir for 5 h to ensure that FeCl3 and MWCNT are fully mixed.
[0117] Step 3, the precursor slurry is placed in a vacuum drying oven at 80°C and dried for 8 hours. After drying, it is placed in a tubular furnace and heated to 350°C at a heating rate of 5°C / min, then kept warm for 30 minutes, and a reducing gas is introduced to heat until the reaction is completed. The tube furnace is cooled to room temperature, and then the powder is taken out to obtain the target product MWCNT-Fe negative electrode-free sodium metal battery electrode material.
[0118] The MWCNT-Fe negative electrode-free sodium metal battery electrode material was mixed with polyvinylidene fluoride at a mass ratio of 9:1, and 1-methyl-2-pyrrolidone solvent was added and ground for 20 minutes before coating on copper foil. After vacuum drying at 120°C, the negative electrode sheet was cut to prepare a negative electrode sheet. A metal sodium sheet was used as the positive electrode, 1M NaPF6 dissolved in ethylene glycol dimethyl ether was used as the electrolyte, and a polypropylene film was used as the separator (PP film) to assemble a composite button cell.
[0119] The battery assembled with the composite electrode material obtained in this embodiment has stable electrochemical performance and long cycle life within the voltage range of 2.5V to 3.8V.
[0120] Comparative Example 1
[0121] The difference between this comparative example 1 and Example 1 is that the mass ratio of MWCNT to sodium-philic metal salt FeCl3 is 1:0, and the other preparation methods are the same. Voltage distribution of constant current sodium electroplating of the battery assembled with the composite electrode material obtained in this comparative example 1 Fig. 9 As shown in the figure, the nucleation overpotential is as high as 22mV, indicating that the nucleation barrier of sodium ion deposition on the electrode sheet is large. The reason for this is that the carbon nanotubes have a large specific surface area and low ion conductivity without the addition of sodium-philic metals, and the active sodium ions are prone to side reactions with the electrolyte. Therefore, it is necessary to add sodium-philic metals to improve the electrochemical performance of the battery.
[0122] Comparative Example 2
[0123] The difference between this comparative example 2 and Example 1 is that the MWCNT is not treated with a dielectric barrier plasma device, and the other preparation methods are the same. The battery assembled with the composite electrode material obtained in this comparative example 1 has a cycle life of 2.5V to 3.8V. Fig.10 As shown in Figure 2, the capacity dropped to 17.3 mAh g after 200 cycles. -1 The reason for this is that the carbon nanotubes have not been treated with a dielectric barrier plasma device, and the metal nuclei are unevenly distributed and easily aggregated, resulting in a greater reaction with active sodium ions, uneven deposition, and high aggregation stress, which easily causes cracks. Therefore, it is necessary to treat CNTs with a dielectric barrier plasma to improve the electrochemical performance of the battery.
[0124] Although the present invention has been described above by combining with exemplary embodiments, it will be apparent to those skilled in the art that various modifications and changes may be made to the exemplary embodiments of the present invention without departing from the spirit and scope defined in the claims.
[0125] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material, characterized in that: The following steps are involved: Step 1, modifying the carbon nanotubes by using a dielectric barrier plasma device; Step 2, mixing and stirring the modified carbon nanotubes with a sodium-philic metal salt to obtain a precursor slurry; Step three, drying the precursor slurry, placing it in a tubular furnace after drying, and introducing a reducing gas to heat the reaction to obtain a carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material.
2. The method for preparing the carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material according to claim 1, characterized in that: The carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material is a porous three-dimensional structure, and the porous three-dimensional structure includes a skeleton formed by the interweaving of the carbon nanotubes and the sodium-philic metal salt uniformly attached to the skeleton.
3. The method for preparing the carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material according to claim 1 or 2, characterized in that: In step 1, the modification treatment of the carbon nanotubes includes placing the carbon nanotubes in a dielectric barrier plasma discharge equipment mold and introducing an inert gas for activation treatment; the inert gas is one or more combinations of argon, nitrogen, and argon-hydrogen mixed gas.
4. The method for preparing the carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material according to claim 1, 2 or 3, characterized in that: In step 2, magnetic stirring is used to obtain the precursor slurry; the speed of the magnetic stirring is 100r / min~300r / min, and the stirring time is 1h~5h; in step 3, the drying treatment is vacuum drying, the vacuum drying time is 10h~24h, and the drying temperature is 40℃~80℃.
5. The method for preparing the carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material according to claim 1, 2 or 3, characterized in that: In step 3, the heating temperature of the heating reaction is increased to 200°C to 500°C at a heating rate of 1°C / min to 10°C / min, and then maintained at 200°C to 500°C for 30min to 5h until the reaction is completed.
6. The method for preparing the carbon nanotube-sodium-philic metal negative electrode-free sodium metal battery electrode material according to claim 1, 2 or 3, characterized in that: The sodium-philic metal salt is one or more combinations of ferric chloride, tin chloride, silver nitrate, magnesium acetate, etc.; the mass ratio of the sodium-philic metal salt to the carbon nanotube is (0-10):
1.
7. A carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material, characterized in that The carbon nanotube-sodium-philic metal anode-free sodium metal battery electrode material is prepared by the method for preparing the carbon nanotube-sodium-philic metal anode-free sodium metal battery electrode material according to any one of claims 1 to 6.
8. A method for preparing a composite electrode sheet for a negative electrode-free sodium metal battery, characterized in that: The following steps are involved: A carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material is mixed with a binder and a solvent to obtain a slurry; the slurry is coated on a negative electrode current collector and dried to obtain a composite electrode sheet; the carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material is prepared by the carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material preparation method as described in any one of claims 1 to 6, or is the carbon nanotube-sodium-philic metal-free negative electrode sodium metal battery electrode material as described in claim 7.
9. The method for preparing a composite electrode sheet for a negative electrode-free sodium metal battery according to claim 8, characterized in that: The coating thickness of the slurry on the negative electrode current collector is 0.001 mm to 0.05 mm.
10. A composite sodium metal battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: The negative electrode is a composite electrode sheet prepared by the method for preparing a composite electrode sheet for a negative electrode-free sodium metal battery as claimed in claim 8 or 9.
Citation Information
Patent Citations
Sodium-philic conductive carbon nanotube framework material, and preparation method and application thereof
CN110577208A
Preparation method of alloy negative electrode material for ultra-long cycle-life sodium ion secondary battery
CN111969192A
Novel sodium-ion battery and method for preparing same
WO2017113234A1
Cited By
Solid electrolyte composite diaphragm, preparation method thereof and negative-electrode-free sodium ion battery
CN121149599A
Negative electrode current collector coating of non-negative electrode sodium metal battery and preparation method of negative electrode current collector coating
CN121306933A