Polyurethane adhesive for use in sandwich panel for 5G radome
By using a special polyurethane adhesive, combining diisocyanate and polyether polyol with high content of oxygen propylene groups, a low Dk and low Df polyurethane adhesive was prepared, which solved the sandwich plate transmission characteristics in the 5G radar radome and The density problem achieves good mechanical performance and low transmission loss.
Patent Information
- Application Number
- CN202380027670.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-15
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-05
AI Technical Summary
Existing polyurethane adhesives have a great impact on the dielectric constant (Dk) and dissipation factor (Df) of sandwich plates in 5G radar radomes, and fail to effectively reduce transmission losses, making it difficult to meet the low Dk and low 5G technology. Df's demand.
Polyurethane adhesives prepared by reacting diisocyanate and/or polyisocyanate with polyether polyol containing at least 50% by weight of oxypropylene group in the presence of chain extenders, crosslinkers, foaming agents, catalysts and additives , a low Dk and low Df adhesive is formed, and an adhesive film is formed between adjacent layers of the sandwich plate.
The low Dk value (≤3.2) and low Df value (≤0.085) of polyurethane adhesive are achieved, while the density of the sandwich plate is reduced (≤1.2g/cm3) and the transmission characteristics and mechanical properties of the 5G radar radome are improved. .
Smart Images

Figure BDA0005042685320000151
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polyurethane adhesives. In particular, the present invention relates to a polyurethane adhesive for preparing a sandwich panel for a 5G radar antenna cover, a sandwich panel for a 5G radar antenna cover prepared therefrom, and a method for preparing the sandwich panel for a 5G radar antenna cover. Background Art
[0002] In recent years, 5G communication technology has developed rapidly. In 5G millimeter wave communication base stations, the wave generally has a wavelength in the millimeter wave band. Due to the short wavelength of such millimeter waves, signal transmission is greatly affected by the material type and structure of the sandwich panels used in the 5G radar antenna cover. Therefore, higher requirements are placed on the materials and structures of the sandwich panels used in the 5G radar antenna cover.
[0003] CN 111421937A describes a laminated material for a 5G millimeter wave radar radome, the laminated material comprising a skin layer and a core layer, wherein the skin layer is made of a thermoplastic resin material and there is an optional adhesive film between the skin layer and the core layer. CN 108091998A describes a V-shaped radar radome obtained by co-curing an antenna, a skin layer and a filling core layer, wherein the skin layer and the filling core layer are bonded together with a cyanate adhesive film. CN104577324A discloses a method for designing a radar radome suitable for a high-power broadband radar, wherein the method includes selecting a material for each layer of a C sandwich structure used in the wall of the radar radome.
[0004] On the other hand, although polyurethane adhesives are well known and widely used, little attention has been paid to their influence on the transmission characteristics of sandwich panels used in 5G radar radomes.
[0005] With the continuous development of 5G technology, there is an urgent need to find a polyurethane adhesive with low transmission loss, especially for use in sandwich panels for 5G radar antenna covers.
[0006] The inventors have surprisingly found that polyurethane adhesives have a significant effect on the dielectric constant (Dk) and dissipation factor (Df) of sandwich panels. Therefore, there is a need to provide such an adhesive, which has a sufficiently low Df combined with a low Dk, while maintaining other advantageous features, such as light weight. Furthermore, there is a need to provide such a sandwich panel for use in 5G radar radomes, which has low transmission losses combined with good mechanical properties. Summary of the invention
[0007] The first object of the present invention is to provide a polyurethane adhesive for use in the preparation of sandwich panels for 5G radar antenna covers, the polyurethane adhesive having a low dissipation factor (Df) of ≤0.085, a low dielectric constant (Dk) of ≤3.2, and a dielectric constant of ≤1.2 g / cm 3 of low density.
[0008] It has now been surprisingly found that the polyurethane adhesives of the present invention provide an optimal balance between transport properties, such as Dk and Df values, and density properties.
[0009] Thus, in one aspect, the presently claimed invention is directed to a polyurethane adhesive formed by:
[0010] (A) diisocyanate and / or polyisocyanate
[0011] (B) a polyol comprising at least one polyether polyol,
[0012] Optionally in
[0013] (C) chain extenders and / or cross-linking agents,
[0014] (D) Foaming agent,
[0015] (E) catalyst and / or
[0016] (F) prepared by reacting in the presence of additives and / or auxiliary agents,
[0017] Wherein the at least one polyether polyol comprises oxypropylene groups in an amount of at least 50 wt %, based on the total weight of the polyether polyol.
[0018] On the other hand, the presently claimed invention relates to the use of the polyurethane adhesive of the invention for producing sandwich panels for use in 5G radar radomes.
[0019] Another aspect of the invention relates to a sandwich panel for a 5G radar antenna cover, wherein the polyurethane adhesive of the invention is present between at least two adjacent layers of the sandwich panel and forms an adhesive film between them, and wherein the sandwich panel has a transmission rate of at least 89% measured at a frequency of 6 GHz according to the ENCHI test method.
[0020] Another object of the present invention is to provide a method for producing a sandwich panel for a 5G radome, wherein at least two adjacent layers of the sandwich panel are bonded by using the polyurethane adhesive according to the present invention. DETAILED DESCRIPTION
[0021] The invention will now be described for purposes of illustration and not limitation.Except in the operating examples or where otherwise indicated, all numbers in the specification expressing amounts, percentages, OH values, functionalities etc. are to be understood as being modified in all instances by the term "about".
[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. As used herein, unless otherwise specified, the following terms have the meanings assigned to them below.
[0023] If a group is defined as comprising at least a certain number of embodiments hereinafter, this means that a group preferably consisting only of these embodiments is also encompassed. In addition, the terms "first", "second", "third" or "(a)", "(b)", "(c)", "(d)" etc. in the specification and claims are used to distinguish between similar elements, and are not necessarily used to describe sequential or chronological order. It should be understood that the terms used in this manner are interchangeable where appropriate, and the embodiments of the present invention described herein can be operated in other sequences different from those described or shown herein. If the terms "first", "second", "third" or "(A)", "(B)" and "(C)" or "(a)", "(b)", "(c)", "(d)", "i", "ii" etc. relate to the steps of method or purposes or determination, there is no time or time interval coherence between these steps, that is, these steps can be performed simultaneously, or there may be a time interval of seconds, minutes, hours, days, weeks, months or even years between such steps, unless otherwise indicated in the present application as described above or below.
[0024] As used herein, the articles "a" and "an" refer to one or to more than one (ie, to at least one) of the grammatical object of the article. By way of example, "an element" means one element or more than one element.
[0025] As used herein, the term "about" should be understood to refer to a range of numbers that one of ordinary skill in the art would consider equivalent to the recited value in the context of achieving the same function or result.
[0026] Unless otherwise indicated, temperature refers to room temperature and pressure refers to ambient pressure. Unless otherwise indicated, all percentages (%) are "weight percents." All values for molecular weight are based on weight average molecular weight, unless otherwise indicated.
[0027] In the following text, different aspects of the present invention are defined in more detail. Each defined aspect can be combined with any other one or more aspects, unless the contrary is clearly indicated. In particular, any feature indicated as preferred or advantageous can be combined with any other one or more features indicated as preferred or advantageous.
[0028] The polyurethane adhesive according to the claimed invention has low Dk and Df values. The Dk and Df values have a great influence on the transmission characteristics of the resulting sandwich panels. Such low Dk and Df values allow sandwich panels with several layers used in 5G radar antenna covers to be bonded together by applying the claimed polyurethane adhesive of the invention to each layer. The polyurethane adhesive according to the present invention typically has a Dk value of ≤3.2, preferably ≤3.1, more preferably 3.0, which is determined by a 2.45 GHz split-column dielectric resonator according to IEC 61189-2-721. The polyurethane adhesive according to the present invention typically has a Df value of ≤0.085, preferably ≤0.081, more preferably ≤0.06, and even more preferably ≤0.05, which is determined by a 2.45 GHz split-column dielectric resonator according to IEC 61189-2-721.
[0029] In addition to having improved Dk and Df values, the polyurethane adhesives of the invention also provide lightness as an additional advantage. For bonding sandwich panels used in 5G radomes, it is crucial to achieve a specific density. It has now been surprisingly found that the claimed polyurethane adhesives of the invention have a reduced density and therefore allow for lightness of the sandwich panels.
[0030] The polyurethane adhesive according to the present invention has a hardness of ≤1.2 g / cm2 measured according to ASTM D1875-03 (2018). 3 , preferably ≤1.15g / cm 3 , more preferably ≤1.12g / cm 3 density.
[0031] According to the present invention, the polyurethane adhesive is prepared by:
[0032] (A) diisocyanate and / or polyisocyanate
[0033] (B) a polyol comprising at least one polyether polyol,
[0034] Optionally in
[0035] (C) chain extenders and / or cross-linking agents,
[0036] (D) Foaming agent,
[0037] (E) catalyst and / or
[0038] (F) prepared by reacting in the presence of additives and / or auxiliary agents,
[0039] Wherein the at least one polyether polyol comprises oxypropylene groups in an amount of at least 50 wt %, based on the total weight of the polyether polyol.
[0040] Suitable details of components (A) through (F) above are provided herein as a guide to prepare a polyurethane adhesive that will have the desired characteristic properties as described above. One of ordinary skill in the art of polyurethane chemistry will appreciate that a wide variety of materials are suitable for these components.
[0041] (A) diisocyanate and / or polyisocyanate
[0042] Diisocyanate and / or polyisocyanate component (A) is an isocyanate functional component that forms a urethane bond when reacting with the hydroxyl groups of the polyol component (B). Suitable diisocyanates and / or polyisocyanates are known to those skilled in the art, and include unmodified isocyanates, modified isocyanates and isocyanate prepolymers. As used herein, the term "polyisocyanate" refers to those containing three or more isocyanate functional groups. Such organic diisocyanates and / or polyisocyanates may include, for example, linear or branched, aliphatic, alicyclic, aromatic, aromatic and heterocyclic polyisocyanates of the type described in W. Siefken, Justus Liebigs Annalen der Chemie, 562, pp. 75 to 136. Examples of such diisocyanates and / or polyisocyanates include those represented by the following formula:
[0043] Q(NCO) n
[0044] wherein n is a number from 2 to 5, preferably from 2 to 3, and Q is: an aliphatic hydrocarbon group containing 2 to 18, preferably from 6 to 10 carbon atoms; an alicyclic hydrocarbon group containing 4 to 15, preferably from 5 to 10 carbon atoms; an aromatic aliphatic hydrocarbon group containing 8 to 15, preferably from 8 to 13 carbon atoms; or an aromatic hydrocarbon group containing 6 to 15, preferably from 6 to 13 carbon atoms.
[0045] Examples of suitable diisocyanates and / or polyisocyanates include, but are not limited to, ethylene diisocyanate; 1,4-tetramethylene diisocyanate; 1,6-hexamethylene diisocyanate; 1,12-dodecane diisocyanate; cyclobutane-1,3-diisocyanate; cyclohexane-1,3- and -1,4-diisocyanate and mixtures of these isomers; 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate); 2,4- and 2,6-hexahydrotoluene diisocyanate and mixtures of these isomers. mixtures of these isomers; dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI or HMDI); 1,3- and 1,4-phenylene diisocyanate; 2,4- and 2,6-toluene diisocyanate and mixtures of these isomers (TDI); diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), mixtures of monomeric diphenylmethane diisocyanates and mixtures of diphenylmethane diisocyanate homologues with a greater number of rings (polymeric MDI); naphthylene-1,5-diisocyanate; triphenylmethane-4,4',4"-triisocyanate; polyphenyl-polymethylene-polyisocyanates (crude MDI) of the type obtainable by condensation of aniline with formaldehyde followed by phosgenation; norbornane diisocyanate; m- or p-isocyanatophenylsulfonyl isocyanate; perchlorinated aryl polyisocyanates; modified polyisocyanates containing carbodiimide groups; modified polyisocyanates containing urethane groups; modified polyisocyanates containing allophanate groups; modified polyisocyanates containing isocyanurate groups; polyisocyanates containing urea groups The invention also includes polyisocyanates containing modified polyisocyanates of 1,2-diuret groups; polyisocyanates containing biuret groups; polyisocyanates obtained by telomerization; polyisocyanates containing ester groups; reaction products of the above isocyanates with acetals; and polyisocyanates containing polymerized fatty acid groups. It is also possible to use isocyanate-containing distillation residues accumulated in the preparation of isocyanates on a commercial scale, optionally in the form of a solution in one or more of the above polyisocyanates. Those skilled in the art will recognize that mixtures of the above polyisocyanates can also be used.
[0046] Isocyanate-terminated prepolymers may also be employed in the present invention. In one embodiment, the isocyanate-terminated prepolymer may be the polymerization product of the corresponding isocyanate itself (i.e., dimer, trimer or oligomer) or the reaction product of an isocyanate component and a component containing an active hydrogen to obtain an isocyanate functionalized prepolymer. Such active hydrogen-containing components have functional groups, such as hydroxyl groups, ester groups or amine groups. In a preferred embodiment, the prepolymer may be prepared by reacting an excess of an organic polyisocyanate or a mixture thereof with a trace amount of an active hydrogen-containing compound (as determined by the well-known Zelvidinov test), as described by Kohler in "Journal of the American Chemical Society," 49, 3181 (1927). These compounds and methods for their preparation are well known to those skilled in the art. The use of any particular active hydrogen-containing compound is not critical; any such compound may be employed in the practice of the present invention.
[0047] Preferably, the diisocyanate and / or polyisocyanate is selected from the group consisting of diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate and one or more isomers or homologs of prepolymers based on diphenylmethane diisocyanate.
[0048] The diisocyanate and / or polyisocyanate component preferably contains such organic diisocyanate and / or polyisocyanate, which has a number average isocyanate (NCO) functionality of at least 1.8 to 4.0, more preferably 2.0 to 3.0, most preferably 2.3 to 2.9. The NCO functionality of the isocyanate component can be a number ranging between (including) any combination of these values. The isocyanate component preferably has a free isocyanate group content (NCO content) in the range of 5 wt % to 50 wt %, more preferably 12 wt % to 40 wt %, most preferably 20 wt % to 35 wt %. The free NCO group content of the polyisocyanate component can be an amount ranging between (including) any combination of these values.
[0049] (B) Polyol
[0050] The polyol according to the claimed invention comprises at least one polyether polyol comprising oxypropylene groups in an amount of at least 50 wt%, based on the total weight of the polyether polyol. In a preferred embodiment, the at least one polyether polyol comprises oxypropylene groups in an amount of at least 70 wt%, preferably at least 80 wt%, and more preferably at least 95 wt%, based on the total weight of the polyether polyol. In addition to the oxypropylene groups, the polyether polyol may comprise oxyethylene groups in an amount of up to 30 wt%, preferably up to 20 wt%, and more preferably up to 10 wt%, based on the total weight of the polyether polyol. It is predicted that polyether polyols comprising oxypropylene groups in an amount of less than 50 wt% may not yield a polyurethane adhesive with desired properties.
[0051] It has been found that the inclusion of at least one polyether polyol in the polyol component has unexpected beneficial effects. The at least one polyether polyol employed in the practice of the present invention typically has an average OH value of 100 mg KOH / g to 650 mg KOH / g, preferably 300 mg KOH / g to 600 mg KOH / g, most preferably 350 mg KOH / g to 500 mg KOH / g and an average functionality of 1.0 to 4.5, preferably 1.5 to 4.0, most preferably 2.5 to 3.2. Preferably, the at least one polyether polyol has an average molecular weight Mw in the range of 90 g / mol to 5000 g / mol, preferably 150 g / mol to 3000 g / mol, more preferably 300 g / mol to 1000 g / mol. The at least one polyether polyol may comprise at least 70 wt % of components (B) to (F) of the present invention, but is generally contained in components (B) to (F) in an amount up to 95 wt %, preferably in an amount of 80 to 90 wt %.
[0052] In a preferred embodiment, the polyol comprises at least one polyether polyol according to the invention. The polyether polyol can be prepared by known processes, for example from one or more alkylene oxides having 2 to 4 carbon atoms in the alkylene moiety by anionic polymerization using alkali metal hydroxides or alkali metal alcoholates as catalysts and adding at least one starter molecule containing 2 to 3 reactive hydrogen atoms, or by cationic polymerization using Lewis acids such as antimony pentachloride or boron fluoride etherate. Examples of suitable alkylene oxides are tetrahydrofuran, 1,3-propylene oxide, 1,2- or 2,3-butylene oxide, and preferably ethylene oxide and 1,2-propylene oxide. Other catalysts that can be used are multimetal cyanide compounds known as DMC catalysts. Alkylene oxides can be used alone, alternately continuously or in the form of a mixture. It is preferred to use a mixture of 1,2-propylene oxide and ethylene oxide, wherein based on the total amount of alkylene oxide, ethylene oxide is used in an amount of up to 20 wt %, and propylene oxide is used in an amount of at least 50 wt %.
[0053] The starting molecule that can be used is water or a diol or triol, such as ethylene glycol, 1,2- or 1,3-propylene glycol, diethylene glycol, dipropylene glycol, 1,4-butylene glycol, glycerol or trimethylolpropane. In another embodiment, molecules with primary and secondary amine functionality can be used as starting materials. Other suitable polyols are polymer-modified polyether alcohols, particularly preferably grafted polyether alcohols. Such polymer-modified polyether polyols are also referred to as polymer polyether alcohols. These polymer polyether alcohols are described by way of example in WO 05 / 098763 and EP-A-250 351, and are usually prepared by free radical polymerization of suitable olefin monomers (such as styrene, acrylonitrile, (meth) acrylate, (meth) acrylic acid and / or acrylamide) in a polyether alcohol used as a grafting base. Side chains are usually generated by free radical transfer from growing polymer chains to polyether alcohols. Apart from graft copolymers, the polymer polyetherols comprise predominantly homopolymers of olefins dispersed in unchanged polyetherol.
[0054] In a preferred embodiment, the monomers used include acrylonitrile or styrene, preferably acrylonitrile and styrene. The monomers are optionally polymerized in a polyether alcohol as a continuous phase in the presence of additional monomers, macromonomers (i.e., unsaturated polyols capable of free radical polymerization) and moderators, and using free radical initiators (mainly azo compounds or peroxide compounds). This process is described by way of example in DE 111 394, US 3 304 273, US 3 383 351, US 3 523 093, DE 1 152 536 and DE 1 152 537.
[0055] During the free radical polymerization, macromonomers are concomitantly incorporated into the copolymer chain. This gives block copolymers with polyether blocks and polyacrylonitrile-styrene blocks; these act as compatibilizers at the interface between the continuous phase and the dispersed phase. The proportion of macromonomers is generally 1% to 20% by weight, based on the total weight of the monomers used to prepare the polymer polyol.
[0056] (C) Chain extender and / or cross-linking agent
[0057] The chain extenders and / or crosslinkers (e) can be used individually or preferably in the form of a mixture. The chain extenders and / or crosslinkers (c) used comprise substances with a molecular weight of preferably less than 500 g / mol, particularly preferably 60 g / mol to 400 g / mol, more preferably 60 g / mol to 250 g / mol, wherein the chain extenders have 2 hydrogen atoms reactive toward isocyanates and the crosslinkers have 3 hydrogen atoms reactive toward isocyanates.
[0058] It is preferred to use simple diols and triols with a molecular weight of less than 400, particularly preferably 60 to 300, and especially 60 to 150. Examples of suitable chain extenders / crosslinkers that can be used include, but are not limited to, ethylene glycol, 1,3-propylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, triethanolamine, triisopropanolamine, tripropylene glycol, diethylene glycol, triethylene glycol, glycerol, and mixtures thereof. The most preferred chain extenders / crosslinkers are liquid at 25°C. Although aliphatic OH functional compounds (such as those just listed) are the most preferred chain extenders / crosslinkers, it is also within the scope of the present invention to employ certain polyamines, polyamine derivatives, and / or polyphenols. Examples of suitable amines known in the art include diisopropanolamine, diethanolamine, and 3,5-diethyl-2,4-diaminotoluene, 3,5-diethyl-2,6-diaminotoluene, and mixtures thereof. Examples of suitable isocyanate-reactive amine derivatives include certain imino-functional compounds such as those described in EP 0 284 253 and EP 0 359 456 and certain enamino-functional compounds such as those having two or more isocyanate-reactive groups per molecule as described in EP 0 359 456. Reactive amines, especially primary aliphatic amines, are less preferred due to their very high reactivity with polyisocyanates, but may optionally be used in minor amounts if desired.
[0059] (D) Foaming agent
[0060] Blowing agent (D) can also be present during the preparation of polyurethane adhesive. Useable blowing agent (D) includes well-known compounds or mixtures of these blowing agents with chemical and / or physical action. Chemical blowing agent is a compound that uses a reaction with isocyanate to form a gaseous product, exemplified by water or formic acid. Physical blowing agent is a compound that has been emulsified or dissolved in the starting material for polyurethane preparation and evaporates under the conditions of polyurethane formation. By way of example, these relate to hydrocarbons, halogenated hydrocarbons and other compounds, for example, perfluorinated alkanes such as perfluorohexane, chlorofluorocarbons and ethers, esters, ketones, acetals and mixtures thereof (for example, alicyclic hydrocarbons with 4 to 8 carbon atoms) or fluorocarbons. Preferred embodiments use a mixture of at least one blowing agent and water comprising the blowing agent as a blowing agent, and particularly use water as the only blowing agent. In a preferred embodiment, the blowing agent may comprise expandable microspheres in the form of hollow polymer microspheres filled with a blowing agent such as a gas or a low boiling liquid, preferably a hydrocarbon. Surprisingly, it has been found that this preferred embodiment makes it possible not only to reduce the density but also to optimize the Dk and Df values of the resulting sandwich panel.
[0061] Expandable microspheres are hollow microspheres that contain a thermoplastic polymer shell (such as polyacrylonitrile or its copolymers) that encapsulates a hydrocarbon gas. When heated, the thermoplastic shell that encapsulates the hydrocarbon gas softens. While the thermoplastic shell softens, the hydrocarbon gas expands and exerts increased pressure on the shell, causing an increase in the volume of the microspheres. The heat to which the material is exposed is sufficient to soften the thermoplastic shell and simultaneously expand the enclosed gas. The expandability of the microspheres can be measured by the TMA density [kg / m 3 ] is indicated by a Mettler Toledo Stare thermal analysis system at a heating rate of 20°C / min. The TMA density here is the minimum density that can be reached at atmospheric pressure before the microspheres collapse. Any heat-expandable microspheres can be used in the present invention. Expandable microspheres containing hydrocarbons, especially aliphatic or alicyclic hydrocarbons are preferred. As used herein, the term "hydrocarbon" is intended to include non-halogenated and partially or completely halogenated hydrocarbons. Examples of expandable microspheres suitable for use in the present invention include, but are not limited to, the EXPANCEL WU, EXPANCEL DU, EXPANCEL SL and EXPANCEL MB series commercially available from AkzoNobel, and ADVANCELL EM commercially available from Sekisui Chemical Company. Other expandable microspheres commercially available or known to those skilled in the art are also suitable for use in the present invention.
[0062] In a preferred embodiment, the blowing agent is used in an amount of 3% to 10% by weight, preferably 4% to 6% by weight, based on the total weight of components (B) to (F).
[0063] (E) Catalyst
[0064] Catalysts for the polyurethane-forming reaction of organic polyisocyanates are well known to those skilled in the art. These catalysts are described by way of example in "Kunststoffhandbuch, Band 7, Polyurethane" [Plastics Handbook, Vol. 7, Polyurethanes] Carl Hanser Verlag, 1993 3rd edition, Chapter 3.4.1. The catalyst, if used, is preferably introduced into the reaction mixture by premixing with the polyol component. As catalyst (F), conventional catalysts as known in the field of polyurethane preparation can be applied. Mention may be made by way of example of amidines such as 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine, tertiary amines such as triethylamine, tributylamine, dimethylbenzylamine, N-methyl-, N-ethyl- and N-cyclohexylmorpholine, N,N,N′,N′-tetramethylethylenediamine, N,N,N′,N′-tetramethylbutanediamine, N,N,N′,N′-tetramethylhexanediamine, pentamethyldiethylenetriamine, tetramethyldiaminoethyl ether, bis(dimethylaminopropyl)urea, dimethylpiperazine, 1,2-dimethylimidazole, 1-azabicyclo[3.3.0]octane and preferably 1,4-diazabicyclo[2.2.2]octane, and also alkanolamine compounds such as triethanolamine, triisopropanolamine, N-methyl- and N-ethyldiethanolamine and dimethylethanolamine. It is also possible to use organometallic compounds, preferably organotin compounds, such as tin(II) salts of organic carboxylic acids, for example tin(II) acetate, tin(II) octoate, tin(II) ethylhexanoate and tin(II) laurate, and dialkyltin(IV) salts of organic carboxylic acids, for example dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate and dioctyltin diacetate; and bismuth carboxylates, such as bismuth(III) neodecanoate, bismuth 2-ethylhexanoate and bismuth octoate; or mixtures thereof. The organometallic compounds can be used alone or preferably in combination with a strongly basic amine. A mixture of a metal catalyst and a basic amine catalyst is optionally used as a catalyst. Preferably, only an amine catalyst is used.
[0065] Preferably, the catalyst is applied in an amount of 0.01% to 2% by weight, preferably 0.1% to 1% by weight, based in each case on the total weight of components (B) to (F).
[0066] (F) Additives and / or auxiliary agents
[0067] For the purposes of the present invention, additives and / or adjuvants may also be used. Preferably, additives and / or adjuvant components are added to the polyol component (B). According to an exemplary embodiment, a portion of the additives and / or adjuvant components are added to the polyol component before the reaction mixture is formed, and another portion is added to the reaction mixture separately. According to another exemplary embodiment, the additives and / or adjuvant components are added to the polyol component in their entirety before the reaction mixture is formed.
[0068] The additive and / or auxiliary component may include, but is not limited to, fillers, water scavengers, degassing agents, surfactants, wetting agents, flame retardants, smoke suppressants, binders, dyes, pigments, hydrolysis inhibitors, antistatic agents, antioxidants, UV stabilizers, trace amounts of inert diluents that reduce viscosity, fungistatic and bacteriostatic substances, combinations of these, and any other known additives from the art. Preferred additives are fillers, water scavengers, degassing agents, binders, UV stabilizers, antioxidants, and / or wetting agents. Additives and / or auxiliary agents can be used to modify the properties of the adhesive, such as controlling wetting behavior, viscosity, shelf life, sag, moisture resistance, etc. The additives used herein are known and are used in the field of polyurethane chemistry to prepare polyurethane adhesives.
[0069] Typically, water scavengers are materials capable of absorbing water. Preferred water scavengers are zeolites and / or calcium oxide. Wetting agents can be used to improve the spreadability of adhesives on the parts to be bonded. Degassing agents can be added to reduce the formation of bubbles or reduce sagging while bonding parts. Preferred fillers are selected from the group consisting of silicon dioxide, titanium dioxide, sulfates, silicates, carbonates, kaolin, chalk, mica, quartz, talc, glass beads, ceramic balls and mixtures thereof. Fillers can be used individually or as a mixture and are advantageously added to the reaction mixture in an amount of 10% to 30% by weight, preferably 15% to 25% by weight, more preferably 15% to 20% by weight, based on the total weight of components (B) to (F).
[0070] To prepare the polyurethane adhesive of the present invention, components (A) to (F) are preferably mixed at a temperature of 15° C. to 70° C., and particularly 20° C. to 50° C. In a preferred embodiment, components (B) to (F) are premixed to form a polyol component, which is then mixed with the isocyanate component (A).
[0071] The stoichiometry of the mixed polyurethane-forming formulation containing organic diisocyanates and / or polyisocyanates and polyol components is usually expressed as an isocyanate index by an amount known in the art. The index of such formulations is simply the equivalent ratio of the sum of the NCO groups of diisocyanates and / or polyisocyanates (A) and the reactive hydrogen atoms of component (B) and optional component (C). This amount is usually multiplied by 100 and expressed as a percentage. The preferred isocyanate index value in the mixed activated formulation suitable for the practice of the present invention ranges from 95 to 150. The more preferred range of the isocyanate index value is from 105 to 130.
[0072] Another object of the present invention is to provide use of the polyurethane adhesive according to the present invention for preparing sandwich panels for use in 5G radar antenna covers.
[0073] Therefore, in one aspect, the present invention provides a sandwich panel for a 5G radar radome, the sandwich panel comprising:
[0074] 1) Inner surface layer,
[0075] 2) at least one first reinforcement layer, the at least one first reinforcement layer covering the inner surface layer;
[0076] 3) a core layer, the core layer covering the at least one first reinforcement layer;
[0077] 4) at least one second reinforcement layer, the at least one second reinforcement layer covering the core layer; and
[0078] 5) an outer layer, the outer layer covering the at least one second reinforcement layer;
[0079] wherein the polyurethane adhesive according to the invention is present between at least two adjacent layers of the sandwich panel and forms an adhesive bond therebetween, and
[0080] The sandwich panel has a transmissivity of at least 89% measured at a frequency of 6 GHz according to the ENCHI test method.
[0081] In a preferred embodiment, the sandwich panel according to the invention has a transmissibility of at least 92%, preferably at least 94%.
[0082] In one embodiment, the inner surface layer and the outer surface layer each have a thickness of 0.2mm to 1mm, and each comprises polycarbonate (PC), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polypropylene (PP) or a combination thereof, preferably PC. In one embodiment, the sandwich panel comprises a third reinforcement layer and a fourth reinforcement layer. In another embodiment, the sandwich panel comprises an additional reinforcement layer. In another embodiment, the first reinforcement layer and the second reinforcement layer (and optionally the third reinforcement layer and the fourth reinforcement layer) each have a thickness of 0.1mm to 0.2mm, and each comprises at least one reinforcing material selected from the group consisting of glass fiber, glass mat, carbon fiber, polyester fiber, aramid fiber, nylon fiber and basalt fiber. In another embodiment, the core layer has a thickness of 2mm to 3mm, and comprises at least one foam selected from the group consisting of polyurethane (PU), polypropylene (PP), polyethylene terephthalate (PET), polystyrene (PS) and polyvinyl chloride (PVC), preferably PU.
[0083] In one embodiment, the polyurethane adhesive according to the present invention is applied to form a bonding film with a thickness of 0.05 mm to 0.3 mm, preferably 0.05 mm to 0.2 mm, more preferably 0.05 mm to 0.1 mm.
[0084] In one embodiment, the sandwich panel according to the invention has a hardness of ≤ 0.9 g / cm2, measured according to ASTM D1875-03 (2018). 3 , preferably ≤0.8g / cm 3 , more preferably ≤0.7g / cm 3 , even more preferably ≤0.65g / cm 3 , and still more preferably ≤0.65g / cm 3 density.
[0085] In one embodiment, the sandwich panel according to the invention has a hardness of ≤ 0.9 g / cm2, measured according to ASTM D1875-03 (2018). 3 , preferably ≤0.8g / cm 3 , more preferably ≤0.7g / cm 3 , even more preferably ≤0.65g / cm 3 , and still more preferably ≤0.65g / cm 3 density.
[0086] In one embodiment, the sandwich panel according to the invention has a thermal conductivity of at least 10 kJ / m2 measured according to IOZD Notched ASTM D256-2010E1. 2 , preferably at least 13KJ / m2 , more preferably at least 14KJ / m 2 , even more preferably at least 15KJ / m 2 , and still more preferably at least 18KJ / m 2 Impact strength.
[0087] In one embodiment, the sandwich panel according to the invention has a thermal conductivity of at least 15 MPa, preferably at least 18 kJ / m 2 , more preferably at least 20KJ / m 2 flexural strength.
[0088] In one embodiment, the sandwich panel according to the invention has a transmissivity of at least 89%, preferably at least 90%, more preferably at least 93% and even more preferably at least 93.5%, measured according to the ENCHI test method at 6 GHz.
[0089] In one embodiment, the sandwich panel according to the invention does not break in a drop ball test, which is performed at a temperature of -40°C with a ball having a weight of 500 g and from a height of 1 meter. The test is performed at a corner of the panel product.
[0090] On the other hand, the present invention also provides a method for preparing a sandwich panel for a 5G radar antenna cover according to the present invention, the method comprising:
[0091] 1) placing at least one first reinforcement layer on the inner surface layer,
[0092] 2) arranging the core layer on the at least one first reinforcement layer,
[0093] 3) placing at least one second reinforcement layer on the core layer, and
[0094] 4) disposing the outer layer on the at least one second reinforcement layer;
[0095] Therein at least two adjacent layers of a sandwich panel are bonded by using the polyurethane adhesive according to the invention.
[0096] The present invention is further illustrated by the following examples but is not limited to the following examples.
[0097] Example
[0098] The following materials were used:
[0099] Polyols
[0100] Polyol 1: Glycerol-started polyoxypropylene polyol with an OH number of 400 mg KOH / g, a hydroxyl functionality of 3 and a molecular weight Mw of 420 g / mol.
[0101] Polyol 2: A glycerol-started polyether polyol comprising propylene oxide units (25.3 wt %) and ethylene oxide units (72.5 wt %) with an OH number of 42 mg KOH / g, a hydroxyl functionality of 2.66 and a molecular weight Mw of 3550 g / mol.
[0102] Polyol 3: A propylene glycol-started polyoxypropylene polyol comprising only propylene oxide units (96.1 wt %) with an OH number of 55 mg KOH / g, a hydroxyl functionality of 1.93 and a molecular weight Mw of 190 g / mol.
[0103] Polyol 4: Propylene glycol-started polyoxypropylene polyol with an OH number of 104 mg KOH / g, a hydroxyl functionality of 1.98 and a molecular weight Mw of 1070 g / mol.
[0104] Crosslinker: Glycerol
[0105] Blowing agent: EXPANCEL DU120 from Nouryon
[0106] Catalyst: POLYCAT SA 8 from Evonik Specialty Chemicals (Shanghai) Co., Ltd.
[0107] Additive 1: addovate LP from BASF
[0108] Additive 2: SILICONE ANTIFOAM from Univa
[0109] Additive 3: Aerosil 200 from Evonik
[0110] Additive 4: Vetec from Sigma-Aldrich (Shanghai) Trading Co., Ltd.
[0111] Isocyanates:
[0112] LUPRANATE M20S from BASF
[0113] Measurement and test methods :
[0114] Dk and Df: IEC 61189-2-721, using 2.45GHz split-pillar dielectric resonator
[0115] Transmission: ENCHI, at 6GHz
[0116] Impact strength: IOZD Notched ASTM D256-2010E1
[0117] Flexural strength: DIN EN ISO 178
[0118] Drop ball test: at -40℃, using a 500g ball and dropping it from a height of 1 meter
[0119] Density: Measured according to ASTM D1875-03(2018) Standard Test Method for Density of Adhesives in Fluid Form
[0120] Examples 1 to 4: Preparation of polyurethane adhesive
[0121] Inventive Examples 1 to 4 were prepared according to the components for forming polyurethane adhesives as specified in Table 1 below. The amounts of the corresponding materials are given in parts by weight. Each of the polyurethane adhesives contained: a B component, which contained a polyol component, a crosslinking agent, a catalyst, a blowing agent, and some additives therein; and an A component, which was an isocyanate.
[0122] The B component is prepared by mixing the corresponding materials as specified in Table 1 by stirring, and then allowing the mixture to stand until the stirring bubbles are removed. The B component thus prepared is then injected into the B tank of the polyurethane low-pressure machine, and the A component is added to the A tank, wherein the temperatures of the B tank and the A tank are set to 20°C to 30°C, respectively. Then, the B component and the A component are mixed for about 1 minute at 2000rpm by a high-speed mixer to obtain the product of the polyurethane adhesive. The cured adhesive is cut for Dk and Df testing. The results are summarized in Table 1 below.
[0123] An epoxy resin adhesive commercially available from Huntsman under the trade name Araldite 2015 was used as a comparative example.
[0124] Table 1
[0125]
[0126] The PO ratio means the weight percentage of oxypropylene groups in the polyether polyol based on the total weight of the polyether polyol.
[0127] Examples 1 to 4 of the present invention achieve the desired compromise Dk and Df values with a value of ≤1.12 g / cm 3 In addition, the Dk value and Df value of the adhesive in Example No. 4 combined with glass fiber (GF) were ≤4.17 and ≤0.04, respectively.
[0128] Preparation of sandwich panels
[0129] A general process for producing a sandwich panel by using the polyurethane adhesive according to the present invention will be described below.
[0130] Example 5: PU foam + GF / epoxy resin + PC
[0131] Epoxy resin adhesives are commercially available under the trade name Araldite 2015 from Huntsman.
[0132] An unrolled PC film with a thickness of 0.75 mm was used as the inner surface layer, on which a glass fiber layer with a thickness of 0.15 mm was set as the first reinforcement layer. Then, a PU foam with a thickness of 2.5 mm as a core layer was set on the glass fiber layer by using an epoxy resin adhesive at a thickness of 0.1 mm. Another glass fiber layer with a thickness of 0.15 mm as a second reinforcement layer was set on the PU foam, and then the other glass fiber layer was covered by a PC film with a thickness of 0.75 mm as an outer surface layer to obtain a 1 mm thick PU foam. 2 The sandwich panels thus prepared were baked at a temperature of 80°C to 90°C with an applied gravity of 20 Kg for 2 hours until fully cured and then cooled to room temperature for property testing. The final thickness was 3.6 mm.
[0133] Example 6: PU foam + GF / PU + PC
[0134] The process of Example 5 was repeated except that the epoxy resin adhesive was replaced by the polyurethane adhesive of Example 4. The final thickness was 3.5 mm.
[0135] The mechanical properties of the sandwich panels prepared above are summarized in Table 2.
[0136] Table 2
[0137] Example 5 Example 6 Thickness, mm 3.6 3.5 Number of layers 5 5 <![CDATA[Density, g / cm 3 > 0.66 0.58 <![CDATA[Impact strength, KJ / m 2 > 15.4 21.9 Transmission rate, % 93.5 94.8 Drop ball test 3 surface marks / no breaks 2 surface marks / no breaks
[0138] The foregoing embodiments of the present invention are provided for the purpose of illustration and not limitation. It will be apparent to those skilled in the art that the embodiments described herein may be modified or altered in various ways without departing from the spirit and scope of the present invention. The scope of the present invention should be determined by the appended claims.
Claims
1. A polyurethane adhesive, the polyurethane adhesive is made by (A) diisocyanate and / or polyisocyanate (B) a polyol comprising at least one polyether polyol, Optionally in (C) chain extenders and / or cross-linking agents, (D) Foaming agent, (E) catalyst and / or (F) prepared by reacting in the presence of additives and / or auxiliary agents, Wherein the at least one polyether polyol comprises oxypropylene groups in an amount of at least 50 wt % based on the total weight of the polyether polyol.
2. The polyurethane adhesive according to claim 1, wherein the polyol contains only the at least one polyether polyol.
3. The polyurethane adhesive according to claim 1 or 2, wherein the at least one polyether polyol comprises oxypropylene groups in an amount of at least 70 wt%, preferably at least 80 wt%, more preferably at least 95 wt%, based on the total weight of the polyether polyol.
4. The polyurethane adhesive according to any one of claims 1 to 3, wherein the at least one polyether polyol further comprises oxyethylene groups in an amount of up to 20 wt%, preferably up to 10 wt%, based on the total weight of the polyether polyol. 5 . The polyurethane adhesive according to claim 1 , wherein the at least one polyether polyol has an average OH value of 100 to 650 mg KOH / g and an average functionality of 1.0 to 4.
5.
6. The polyurethane adhesive according to any one of claims 1 to 5, wherein the blowing agent comprises expandable microspheres in the form of hollow polymer microspheres filled with a blowing agent such as a gas or a low boiling point liquid, preferably a hydrocarbon.
7. The polyurethane adhesive according to claim 6, wherein the foaming agent is used in an amount of 3 to 10 wt% based on the total weight of components (B) to (F).
8. The polyurethane adhesive according to any one of claims 1 to 5, wherein the additives and / or auxiliary agents comprise at least one filler selected from the group consisting of silicon dioxide, titanium dioxide, sulfates, silicates, carbonates, kaolin, chalk, mica, quartz, talc, glass beads, ceramic balls and mixtures thereof.
9. The polyurethane adhesive according to claim 8, wherein the filler is used in an amount of 10 to 30 wt% based on the total weight of components (B) to (F).
10. The polyurethane adhesive according to any one of claims 1 to 9, wherein (A) diisocyanate and / or polyisocyanate is combined with the total of (B) polyol and (C) chain extender and / or crosslinker in an amount such that the isocyanate index is in the range of 95 to 120.
11. Use of the polyurethane adhesive according to any one of claims 1 to 10 for producing sandwich panels for use in 5G radar radomes.
12. A sandwich panel for a 5G radar antenna cover, the sandwich panel include: 1) Inner surface layer, 2) at least one first reinforcement layer, the at least one first reinforcement layer covering the inner surface layer; 3) a core layer, the core layer covering the at least one first reinforcement layer; 4) at least one second reinforcement layer, wherein the at least one second reinforcement layer covers the core layer; as well as 5) an outer layer, the outer layer covering the at least one second reinforcement layer; wherein the polyurethane adhesive according to any one of claims 1 to 10 is present between at least two adjacent layers of the sandwich panel and forms an adhesive bond therebetween, and The sandwich panel has a transmissivity of at least 89% measured at a frequency of 6 GHz according to the ENCHI test method.
13. The sandwich panel for a 5G radome according to claim 12, wherein the sandwich panel has a transmission rate of at least 92%, preferably at least 94%.
14. The sandwich panel for a 5G radar antenna cover according to claim 12 or 13, wherein the inner surface layer and the outer surface layer each have a thickness of 0.2 mm to 1 mm, and each comprises polycarbonate (PC), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polypropylene (PP) or a combination thereof, preferably PC.
15. The sandwich panel for a 5G radar antenna cover according to claim 12 or 13, wherein the first reinforcement layer and the second reinforcement layer each have a thickness of 0.1 mm to 0.2 mm, and each contain at least one reinforcement material selected from the group consisting of glass fiber, glass mat, carbon fiber, polyester fiber, aramid fiber, nylon fiber and basalt fiber.
16. The sandwich panel for a 5G radar antenna cover according to claim 12 or 13, wherein the core layer has a thickness of 2 to 3 mm and comprises at least one foam selected from the group consisting of polyurethane (PU), polypropylene (PP), polyethylene terephthalate (PET), polystyrene (PS) and polyvinyl chloride (PVC), preferably PU.
17. A method for preparing a sandwich panel for a 5G radar antenna cover according to any one of claims 12 to 16, the method include: 1) placing at least one first reinforcement layer on the inner surface layer, 2) arranging the core layer on the at least one first reinforcement layer, 3) arranging at least one second reinforcement layer on the core layer, and 4) disposing the outer layer on the at least one second reinforcement layer; Wherein at least two adjacent layers of the sandwich panel are bonded by using the polyurethane adhesive according to any one of claims 1 to 10.
Citation Information
Patent Citations
Method for designing large-power-resisting broadband radar antenna cover
CN104577324A
V-shaped radar radome structure and preparation method thereof
CN108091998A
Composite material for 5G millimeter wave radome and preparation method thereof
CN111421937A
Isocyanate reactive polymers having imino / enamine functionality
EP0359456A1
Method of preparing polyurethanes from liquid, stable, reactive, filmforming polymer / polyol mixtures formed by polymerizing an ethylenically unsaturated monomer in a polyol
US3304273A