R-t-b sintered magnet
By adjusting the content of rare earth elements and diffusion of metal elements, the B/T ratio of the sintered magnet of R-T-B system is optimized, and the problems of HcJ reduction and Tb supply instability at high temperatures are solved, and the magnet performance of high Br and high HcJ is achieved, which is suitable for electric vehicles. and other fields.
Patent Information
- Application Number
- CN202380028890.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2023-02-22
- Publication Date
- 2024-11-05
AI Technical Summary
The existing R-T-B system sintered magnets have reduced coercive force HcJ at high temperatures, resulting in irreversible thermal demagnetization problems. At the same time, the use of heavy rare earth elements such as Tb has unstable supply and price fluctuations, making it difficult to simultaneously increase the residual magnetic flux density Br and HcJ.
By adjusting the contents of Nd, Pr, Ce, La, Dy, and Tb in the R-T-B system sintered magnet, and diffusing metal elements such as Ga, Cu, Zn, Al, and Si to the inside of the magnet surface, the B/T atomic ratio is controlled to be low. On 1/14, a low-boron R-T-B system sintered body is formed to promote the grain boundary diffusion of R and metal elements and optimize the magnet characteristics.
While reducing the use of heavy rare earth elements, it also increases the residual magnetic flux density Br and coercive force HcJ, and obtains high-performance R-T-B-type sintered magnets to meet the needs of electric vehicles and other fields.
Smart Images

Figure CN118901108A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a RTB-based sintered magnet. Background Art
[0002] RTB-based sintered magnets (R is at least one of the rare earth elements, T is Fe or Fe and Co, and B is boron) are considered to be the magnets with the highest performance among permanent magnets. Therefore, RTB-based sintered magnets are used in various engines in the automotive field such as electric vehicles (EV, HV, PHV), renewable energy fields such as wind power generation, home appliance fields, and industrial fields. RTB-based sintered magnets are indispensable materials for the miniaturization / lightweight, high efficiency / energy saving (improvement of energy efficiency) of these engines. In addition, by using RTB-based sintered magnets in drive motors for electric vehicles, replacing internal combustion engine vehicles with electric vehicles will also help prevent global warming by reducing greenhouse gases such as carbon dioxide (reduction of fuel gas / exhaust gas). RTB-based sintered magnets have made a significant contribution to the realization of a clean energy society.
[0003] RTB sintered magnets are mainly composed of R2T 14 The main phase of the B-type compound and the grain boundary phase located at the grain boundary of the main phase. 14 B-type compounds are ferromagnetic materials with high saturation magnetization (intensity) and anisotropic magnetic field, which determine the characteristics of RTB-based sintered magnets.
[0004] RTB sintered magnets have a coercive force H at high temperature. cJ (hereinafter sometimes referred to as "H cJ ”) is reduced, and there is a problem of irreversible thermal demagnetization. For this reason, the RTB-based sintered magnets used in electric vehicle engines are required to have high H even at high temperatures. cJ , that is, it has a higher H at room temperature cJ .
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2007 / 102391
[0008] Patent Document 2: International Publication No. 2018 / 143230 Summary of the invention
[0009] Technical problem to be solved by the invention
[0010] It is known that when heavy rare earth elements RH (mainly Tb and Dy) replace R2T 14When the light rare earth elements RL (mainly Nd and Pr) in B-type compounds, H cJ But there is one aspect that increases H cJ On the other hand, due to R2T 14 The saturation magnetization of the B-type compound phase decreases, causing the residual magnetic flux density B r (hereinafter referred to as “B r In addition, due to the limited amount of Tb resources and the limited production areas, Tb has problems such as unstable supply and price fluctuations. Therefore, a method that can suppress B without using Tb as much as possible (reducing the amount used as much as possible) is needed. r The reduction and high H cJ technology.
[0011] Patent Document 1 describes a method for supplying a heavy rare earth element RH to the surface of a sintered magnet of an RTB alloy and simultaneously diffusing the heavy rare earth element RH into the interior of the sintered magnet. The method described in Patent Document 1 allows the heavy rare earth element RH to diffuse from the surface of the RTB sintered magnet into the interior, thereby concentrating the heavy rare earth element RH in a region that can effectively increase the H cJ The outer shell of the main phase grains can inhibit B r of the decrease and obtain a high H cJ .
[0012] Patent document 2 records that the light rare earth elements RL and Ga diffuse from the surface of the RTB-based sintered body through the grain boundary into the interior of the magnet together with the heavy rare earth element RH. The method described in patent document 2 can promote the diffusion of the heavy rare earth element RH into the interior of the magnet, thereby reducing the amount of heavy rare earth element RH used while obtaining extremely high H cJ .
[0013] In recent years, especially in the field of electric vehicle engines, it is necessary to reduce the amount of heavy rare earth elements RH, especially Tb, and obtain higher B r and high H cJ .
[0014] Various embodiments of the present invention provide a method for reducing the use of heavy rare earth elements RH such as Tb while having high B r and high H cJ RTB sintered magnet.
[0015] Technical solutions for solving technical problems
[0016] The RTB system sintered magnet of the present invention, in a non-limiting exemplary embodiment, is an RTB system sintered magnet (R is at least one of the rare earth elements and must contain Nd, T is Fe or Fe and Co, and B is boron), including R2T 14 The main phase of the B-type compound and the grain boundary phase located in the grain boundary portion of the above-mentioned main phase, when the content (mass %) of Nd is [Nd], the content (mass %) of Pr is [Pr], the content (mass %) of Ce is [Ce], the content (mass %) of La is [La], the content (mass %) of Dy is [Dy], the content (mass %) of Tb is [Tb], the content (mass %) of B is [B], the content (mass %) of O is [O], the content (mass %) of C is [C], and the content (mass %) of M (M is at least one selected from Ga, Cu, Zn, Al and Si) is [M], the atomic ratio of B to T in the RTB based sintered magnet is lower than R2T 14 The stoichiometric composition of the B-type compound is the ratio of the number of atoms of B to T, and satisfies the relationships of 26.0 mass%≤([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≤27.7 mass%, 0.85 mass%≤[B]≤0.94 mass%, 0.05 mass%≤[O]≤0.30 mass%, 0.05 mass%≤[M]≤2.00 mass%, [Tb]≤0.20 mass% and [Dy]≤0.30 mass%, including a portion in which at least one of the Nd concentration and the Pr concentration gradually decreases from the surface of the magnet to the inside of the magnet.
[0017] In one embodiment, the portion where the M concentration gradually decreases from the surface of the magnet toward the inside of the magnet is included.
[0018] In one embodiment, the portion where the Pr concentration gradually decreases from the surface of the magnet toward the inside of the magnet is included.
[0019] In one embodiment, 0.85 mass % ≤ [B] ≤ 0.92 mass %.
[0020] In one embodiment, 0.05 mass % ≤ [Tb] ≤ 0.20 mass %, the residual magnetic flux density (B r ) is above 1.43T, the coercive force (H cJ ) is above 1900kA / m.
[0021] In one embodiment, Tb is not contained (except for unavoidable impurities), and the residual magnetic flux density (B r ) is above 1.40T, the coercive force (H cJ ) is above 1400kA / m, and when Br Set the value of (T) to [Y], H cJ When the value (kA / m) is set to [X], the relationship [Y]≥-0.0002×[X]+1.73 is satisfied.
[0022] In one embodiment, the RTB based sintered magnet contains Ga and Cu, and when the Ga content (mass %) is [Ga] and the Cu content (mass %) is [Cu], [Ga]≥1.2×[Cu].
[0023] Effects of the Invention
[0024] According to the embodiment of the present invention, it is possible to provide a device which reduces the usage of heavy rare earth elements RH such as Tb and has high B r and high H cJ RTB sintered magnet. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1A It is a schematic cross-sectional view showing a part of an enlarged RTB based sintered magnet.
[0026] Figure 1B Yes means Figure 1A A schematic cross-sectional view of the further enlarged dashed rectangular area.
[0027] Figure 2A 1 is a schematic perspective view showing an RTB based sintered magnet 100 according to an embodiment of the present invention.
[0028] Figure 2B This is a graph showing an example of a portion of the RTB based sintered magnet 100 where at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface toward the inside of the magnet.
[0029] Figure 3 This is a flow chart showing an example of the process of the method for producing an RTB based sintered magnet according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] First, the basic structure of the RTB based sintered magnet of the present invention is described. The RTB based sintered magnet has a structure in which powder particles of a raw material alloy are bonded by sintering, and is mainly composed of R2T 14 The main phase of the B compound particles and the grain boundary phase located in the grain boundary portion of the main phase are formed.
[0031] Figure 1A It is a schematic cross-sectional view showing a partially enlarged portion of an RTB-based sintered magnet. Figure 1B Yes means Figure 1A A further enlarged cross-sectional view of the dotted rectangular area. Figure 1A In the figure, as an example, an arrow with a length of 5 μm is recorded, and it is used as a reference length for indicating the size. Figure 1A and Figure 1B As shown in the figure, RTB sintered magnets are mainly composed of R2T 14 The main phase 12 of the B compound and the grain boundary phase 14 located at the grain boundary of the main phase 12 are composed. Figure 1B As shown, the grain boundary phase 14 includes two R2T 14 The two adjacent grain boundary phases 14a and three R2T 14 The grain boundary triple junction 14b is where the B compound grains are adjacent to each other. The typical main phase grain size is 3 μm or more and 10 μm or less in terms of the average value of the equivalent circle diameter of the magnet cross section. The R2T of the main phase 12 is 14 B compound is a ferromagnetic material with high saturation magnetization (intensity) and anisotropic magnetic field. Therefore, in RTB based sintered magnets, by increasing the R2T 14 The presence ratio of B compounds can increase the r To improve R2T 14 The ratio of the B compound is preferably such that the R content, T content, and B content in the raw material alloy are close to R2T 14 The stoichiometric ratio of the B compound (R content: T content: B content = 2:14:1).
[0032] However, since the RTB based sintered magnet also has a grain boundary phase 14, the R, T, and B in the raw material alloy are not only used for the main phase 12, but also consumed in the formation of the grain boundary phase 14. The grain boundary phase 14 melts during the sintering process and makes the R2T 14 The B compounds are physically bonded to each other. Therefore, the grain boundary phase 14 is designed to be a rare earth-rich (R-rich) composition with a relatively low melting temperature. Specifically, the composition of the raw alloy is set to have an R content greater than R2T 14 On the other hand, it is known that the composition of the grain boundary phase 14, specifically the type and amount of substances contained in the grain boundary phase 14, will affect the H cJ size.
[0033] As described above, in the method disclosed in Patent Document 2, R and Ga diffuse from the surface of the RTB-based sintered body into the interior of the magnet through the grain boundaries. R and Ga diffused to the grain boundaries diffuse into the interior of the magnet, which can achieve high H cJ However, according to the research results of the inventors of the present invention, once R and Ga diffuse into the interior of the magnet, the grain boundary phases of the two grains will become too thick, and the volume ratio of the main phase will decrease, resulting in B rTherefore, it can be seen that the diffusion amount of R and Ga should be kept to the minimum necessary so that the grain boundary phase between the two grains does not become too thick.
[0034] In addition, the ratio of the number of atoms of B to T (B / T) contained in the RTB system sintered magnet is lower than that of the R2T 14 The atomic ratio of B to T in the stoichiometric composition of the B compound can reveal changes in the composition of the grain boundary phase (the types and concentrations of substances such as iron-based compounds and rare earth compounds that may exist in the grain boundaries).
[0035] The inventors of the present invention have found that the atomic ratio of B to T (B / T) contained in RTB based sintered magnets is lower than that in R2T 14 When the atomic ratio of B to T in the stoichiometric composition of the B compound is 1 / 14, the effect of improving the magnetic properties brought about by the grain boundary diffusion of R and Ga is enhanced. That is, when the atomic ratio of B / T is lower than 1 / 14, the grain boundary diffusion of R and Ga is promoted. It should be noted that in the case of R2T 14 In the B compound, even if part of B is replaced by carbon (C), the same effect can be achieved. It is also known that the magnetic properties can be improved when at least one selected from Cu, Zn, Al and Si is diffused instead of Ga or on the basis of Ga. Hereinafter, one or more metals selected from Ga, Cu, Zn, Al and Si are collectively referred to as metal elements M.
[0036] In this way, when R and metal element M diffuse from the surface to the inside of the RTB system sintered body, the atomic ratio of B / T is one of the important parameters for adjusting the grain boundary diffusion behavior and improving the magnet properties. Hereinafter, RTB system sintered bodies and RTB system sintered magnets with a B / T atomic ratio lower than 1 / 14 are sometimes referred to as "low-boron RTB sintered bodies" and "low-boron RTB system sintered magnets", respectively. It should be noted that in the present invention, the RTB system sintered magnet before and during diffusion is referred to as "RTB system sintered body", and the RTB system sintered magnet after diffusion is referred to as "RTB system sintered magnet".
[0037] The inventors of the present invention have further studied and found that: the main phase R2T is replaced 14 The C of B in the B compound combines with the rare earth oxide in the grain boundary through the sintering process to form a rare earth oxygen carbon compound (ROC compound) in the grain boundary. It is also shown that the atomic ratio in this case is R: (C, O) = 1: 1. Once this ROC compound is generated at the grain boundary, it constitutes the main phase R2T 14 The C content of B compound is reduced accordingly. As mentioned above, even if R2T 14The effect of "low boron" can also be obtained by replacing part of B in the B compound with C. Therefore, the main phase R2T 14 The reduction of the C content of the B compound will effectively reduce the total amount of B and C. In addition, the formation of ROC compounds at the grain boundaries means that part of the rare earth element R contained in the raw alloy is consumed by the formation of ROC compounds. It should be noted that ROC compounds include RO compounds (rare earth oxides) and RC compounds (rare earth carbides).
[0038] Based on the above, the inventors of the present invention believe that in order to optimize the improvement effect of magnetic properties brought about by diffusion when R or metal element M diffuses from the surface of a low-boron RTB-based sintered body to the inside, it is necessary to control the thickness and structure of the grain boundary, and for this purpose, the contents of R, O and C need to satisfy an appropriate relationship. Moreover, the inventors also believe that such R having an appropriate relationship with the contents of O and C can enhance the effect of improving magnetic properties brought about by the grain boundary diffusion of R and M by containing a low content of boron in a specific range. Moreover, the research results show that when R and / or metal element M are diffused into the RTB-based sintered body, R and M will not diffuse excessively into the interior of the magnet, but can form an appropriate two-grain grain boundary, wherein the above-mentioned RTB-based sintered body is set to [Nd] with a content (mass %) of Nd, [Pr] with a content (mass %) of Ce, [Ce] with a content (mass %) of La, [La] with a content (mass %) of Dy. When the content (mass %) of [Dy], the content (mass %) of Tb, the content (mass %) of B, the content (mass %) of O, and the content (mass %) of C are set to [C], the content is adjusted to a range of 0.85 mass % ≤ [B] ≤ 0.94 mass % and 25.8 mass % ≤ ≤ ([Nd] + [Pr] + [Ce] + [La] + [Dy] + [Tb]) - 12 ([O] + [C]) ≤ 27.5 mass %. In the RTB system sintered magnet thus obtained, the atomic ratio of B to T in the RTB system sintered magnet is lower than R2T. 14 The ratio of the number of atoms of B to T in the stoichiometric composition of the B compound satisfies
[0039] 26.0 mass%≤([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≤27.7 mass%,
[0040] 0.85 mass%≤[B]≤0.94 mass%,
[0041] 0.05 mass%≤[O]≤0.30 mass%,
[0042] 0.05 mass% ≤ [M] ≤ 2.00 mass%,
[0043] the relationship of [Tb] ≤ 0.20 mass% and [Dy] ≤ 0.30 mass%.
[0044] Hereinafter, the R-T-B type sintered magnet of the embodiment of the present invention will be described in detail.
[0045] <R-T-B type sintered magnet>
[0046] The R-T-B type sintered magnet of the present invention includes a main phase containing an R2T 14 B compound and a grain boundary phase located at the grain boundary portion of the main phase. This R-T-B type sintered magnet includes a portion where at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface toward the magnet interior. The portion where at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface toward the magnet interior is formed by the diffusion of at least one of Nd and Pr from the magnet surface toward the magnet interior. Details of this will be described later.
[0047] Let the content (mass%) of Nd in the R-T-B type sintered magnet of the embodiment of the present invention be [Nd], the content (mass%) of Pr be [Pr], the content (mass%) of Ce be [Ce], the content (mass%) of La be [La], the content (mass%) of Dy be [Dy], the content (mass%) of Tb be [Tb], the content (mass%) of T be [T], the content (mass%) of B be [B], the content (mass%) of O be [O], the content (mass%) of C be [C], and the content (mass%) of the metal element M be [M]. These contents may be 0 mass% or a value below the measurement limit when there is no particularly specified lower limit value. In other words, the R-T-B type sintered magnet of the present embodiment may, for example, not contain Ce, La, Tb, and / or Dy.
[0048] As described above, in the R-T-B type sintered magnet of the present embodiment, the atomic number ratio of B to T is lower than the atomic number ratio of B to T in the stoichiometric composition of the R2T 14 B compound. If this ratio is expressed as a mass ratio (ratio of mass% (mass%) rather than an atomic number ratio), it is expressed by the following formula (1) (since T is an iron-based element, the atomic number of Fe is used).
[0049] [T] / 55.85 > 14 × [B] / 10.8 (1)
[0050] In the RTB based sintered magnet of this embodiment, the oxygen content range is defined by 0.05 mass % ≤ [O] ≤ 0.30 mass %. This level of oxygen content can be achieved by controlling the oxidation conditions when preparing the coarse pulverized powder (hydrogen pulverized powder) or fine pulverized powder of the raw material alloy. This will be described later.
[0051] In the RTB based sintered magnet of the present embodiment, the following formula (2) holds true.
[0052] 26.0 mass%≤([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≤27.7 mass%(2)
[0053] That is, in this embodiment, the contents of R (R is at least one of the rare earth elements and must contain Nd), O and C in the RTB-based sintered body are adjusted to satisfy the above formula (2). It should be noted that the C content can be adjusted by the amount of lubricant added during crushing or molding. Preferably, the content of formula 2 is 26.0 mass% or more and 27.5 mass% or less. It is possible to further reduce the amount of heavy rare earth elements RH such as Tb, while obtaining a high B r and H cJ .
[0054] The above formula (2) represents the effective rare earth element content range in R of the RTB system sintered magnet, excluding the elements mixed into the grain boundary phase due to bonding with O or bonding with C. The main component of the rare earth elements contained in the RTB system sintered magnet is Nd. Therefore, Nd can be selected as a representative of Nd, Pr, Ce, La, Dy, and Tb, and the substitution main phase R2T can be selected. 14 The C of B in the B compound is used as a representative of O and C, and the weight ratio of the rare earth elements consumed is estimated. The atomic weights of Nd and C are approximately 144 and 12, respectively. Therefore, by combining with 1.0 mass% of [C], 144 / 12=12.0 mass% of [Nd] will be consumed. Thus, the above formula (2) approximately represents the amount of rare earth elements remaining after removing the rare earth elements consumed by combining with C or O from the rare earth elements (Nd, Pr, Ce, Dy, Tb).
[0055] In the present invention, ([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12×([O]+[C]) is sometimes referred to as the R' amount. The above formula (2) defines the R' amount to be in the range of 26.0 mass % or more and 27.7 mass % or less. It can be seen that when the R' amount is less than 26.0 mass %, it is difficult for R and M to be supplied from the surface of the magnet to the inside, and H cJ It can also be seen that when the amount of R' is higher than 27.7 mass%, R and the like may diffuse excessively from the surface of the magnet to the interior of the magnet, and Br When it is within this range, it can have a higher B r and higher H cJ .
[0056] The Tb content in the RTB-based sintered magnet of the present embodiment is [Tb]≤0.20% by mass, and the Dy content is [Dy]≤0.30% by mass. As a result of adjusting the oxygen content within the above range and controlling R to satisfy the above formula (2), metal elements M and R such as Ga will not diffuse excessively into the interior of the magnet, and even if the Tb and Dy contents are small, the desired excellent magnet properties can be achieved.
[0057] Since at least one of Nd and Pr diffuses from the magnet surface to the inside of the magnet in the RTB based sintered magnet of this embodiment, the result includes a portion where at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface to the inside of the magnet.
[0058] Figure 2A 1 is a schematic perspective view showing an RTB based sintered magnet 100 according to the present embodiment. Figure 2B This is a graph showing an example of a portion of the RTB based sintered magnet 100 where at least one of the Tb concentration and the Dy concentration gradually decreases from the magnet surface toward the inside of the magnet. Figure 2A , mutually orthogonal X-axis, Y-axis, and Z-axis are shown for reference.
[0059] exist Figure 2A In the example shown, the RTB based sintered magnet 100 has an upper surface 100T and a lower surface 100B corresponding to a part of the magnet surface, and a side surface 100S. The dimension of the RTB based sintered magnet 100 in the Z-axis direction is a thickness t. Figure 2B In the graph of , the vertical axis is the depth (Z) from the upper surface T of the RTB system sintered magnet 100, and the horizontal axis represents the concentration (D) of at least one of the Nd concentration and the Pr concentration. In this example, Pr diffuses into the magnet through the upper surface 100T and the lower surface 100B of the RTB system sintered magnet 100. The result is shown in FIG. Figure 2B As shown, as viewed from the center of the magnet, the portion where the Pr concentration gradually decreases from the magnet surface toward the inside of the magnet exists in two parts, the upper surface 100T side and the lower surface 100B side.
[0060] Next, the meaning of the RTB system sintered magnet including a portion where at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface to the magnet interior is explained. As described above, the RTB system sintered magnet including a portion where at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface to the magnet interior means that at least one of Nd and Pr is in a state of diffusion from the magnet surface to the magnet interior. This state can be confirmed by, for example, energy dispersive X-ray spectroscopy (EDX) of an arbitrary cross section of the RTB system sintered magnet from the magnet surface to the vicinity of the center of the magnet.
[0061] When the size of the measurement site is, for example, submicron-level, the concentrations of Nd and Pr are increased as the measurement site is located in the main phase grain (R2T 14 In addition, when the measurement site is located at the grain boundary, the concentration of Nd or Pr will change locally or microscopically depending on the type and distribution of compounds containing Nd or Pr that will be formed at the grain boundary. However, in the case where Nd and Pr diffuse from the surface of the magnet to the inside of the magnet, the average concentration of these elements at positions at the same depth from the surface of the magnet is obviously in a state of gradually decreasing from the surface of the magnet to the inside of the magnet. In the present invention, at least in the area from the magnet surface to a depth of 200μm of the RTB system sintered magnet, when at least one of the average concentrations of Nd and Pr measured as a function of depth as a parameter decreases with increasing depth, the RTB system sintered magnet is defined as containing a portion in which at least one of the Nd concentration and the Pr concentration gradually decreases.
[0062] In the manufacturing process of the RTB system sintered magnet of this embodiment, not only at least one of Nd and Pr but also preferably a metal element M (M is at least one selected from Ga, Cu, Zn, Al and Si) diffuses from the magnet surface to the inside of the magnet. Therefore, in a more preferred embodiment, the RTB system sintered magnet includes a portion where the concentration of the element M (M is at least one selected from Ga, Cu, Zn, Al and Si) gradually decreases from the magnet surface to the inside of the magnet.
[0063] The portion containing at least one of Nd and Pr and the metal element M whose concentration gradually decreases from the magnet surface to the magnet interior means that these elements are in a state of diffusing from the magnet surface to the magnet interior. Whether or not "the portion containing the specified element whose concentration gradually decreases from the magnet surface to the magnet interior" can be confirmed by, for example, line analysis (line analysis) of any cross section of the RTB system sintered magnet from the magnet surface to the vicinity of the magnet center) by energy dispersive X-ray spectroscopy (EDX). The concentration of these specified elements will be determined by the measurement site being the main phase grain (R2T 14B compound particles) or grain boundaries, or RTB system sintered magnets before diffusion, and the types and presence or absence of compounds containing R and metal element M produced during diffusion. However, the overall concentration gradually decreases as you go deeper into the magnet (the concentration gradually decreases). Therefore, even if the local concentration of the specified element decreases or increases, it can be identified as "the portion containing the specified element whose concentration gradually decreases from the surface of the magnet to the inside of the magnet" belonging to the present invention.
[0064] The RTB based sintered magnet of this embodiment may have, for example, the following composition.
[0065] R: 26.8 mass % or more and 31.5 mass % or less (R is at least one of the rare earth elements and must contain Nd),
[0066] B: 0.85 mass % or more and 0.94 mass % or less,
[0067] M: 0.05 mass % or more and 2.0 mass % or less (M is at least one selected from Ga, Cu, Zn, Al and Si),
[0068] Q: 0 mass% or more and 2.0 mass% or less (Q is at least one selected from Ti, V, CR1-Mn, Ni, Zr, Nb, Mo, Ag, In, Sn, Hf, Ta, W, Pb and Bi),
[0069] The remainder is T (T is Fe or Fe and Co) and inevitable impurities.
[0070] In addition to Nd, R may include La, Ce, Pr, Pm, Sm, Eu, etc. Usually, O (oxygen), N (nitrogen), C (carbon), etc. are also contained as inevitable impurities, but in the embodiment of the present invention, the behavior of O and C is particularly focused on, and the relationship between their content and the content of the specified rare earth element is specified, thereby successfully achieving high B r and H cJ When the content of B is [B] (mass %), preferably, 0.85 mass % ≤ [B] ≤ 0.92 mass %. This can obtain a higher H cJ .
[0071] The RTB based sintered magnet preferably contains M1 (M1 is at least one selected from Ga, Zn and Si), and when the Ga content (mass %) is [Ga], the Zn content (mass %) is [Zn], and the Si content (mass %) is [Si], 0.35 mass % ≤ [M1] ≤ 1.00 mass %. By satisfying the above formula 2 and B in a specific range and setting M1 to 0.35 mass % or more and 1.00 mass % or less, a higher H can be obtained. cJ。
[0072] Preferably, the R-T-B-based sintered magnet contains Ga. When the content of Ga (mass %) is [Ga], it is 0.40 mass % ≤ [Ga] ≤ 0.80 mass %. By satisfying the above formula 2 and B within a specific range, and making Ga be 0.40 mass % or more and 0.80 mass % or less, a higher H can be obtained. cJ More preferably, the R-T-B-based sintered magnet contains Ga and Cu. When the content of Ga (mass %) is [Ga] and the content of Cu (mass %) is [Cu], [Ga] ≥ 1.2 × [Cu], and a higher H can be obtained. cJ 。
[0073] In an embodiment of the present invention, an R-T-B-based sintered magnet can be obtained that not only reduces the usage amount of heavy rare earth elements RH such as Tb, but also has a high B r and a high H cJ Typically, when (mass %) is set as [B], it is 0.05 ≤ [Tb] ≤ 0.20 mass %, the remanent flux density (B r ) is 1.43 T or more, and the coercivity (H cJ ) is 1900 kA / m or more. Additionally, it is preferably free of Tb (except for inevitable impurities), the remanent flux density (B r ) is 1.40 T or more, the coercivity (H cJ ) is 1400 kA / m or more, and when the value (T) of B r is set as [Y] and the value (kA / m) of H cJ is set as [X], the relationship of [Y] ≥ -0.0002 × [X] + 1.73 is satisfied. Satisfying the relationship of [Y] ≥ -0.0002 × [X] + 1.73 means that high magnetic properties with both excellent B r and H cJ can be obtained.
[0074] <Method for manufacturing R-T-B-based sintered magnet>
[0075] The following describes an embodiment of the method for manufacturing the R-T-B-based sintered magnet of the present invention.
[0076] The manufacturing method of this embodiment is as Figure 3As shown, it may include step S10 of preparing an RTB system sintered body, step S20 of preparing an R1-M alloy, step S30 of performing a first heat treatment, and step S40 of performing a second heat treatment. Step S30 is a step of performing a first heat treatment at a temperature of 700°C to 950°C in a vacuum or inert gas environment by bringing at least a portion of the R1-M alloy into contact with at least a portion of the surface of the RTB system sintered body, thereby diffusing R1 and M into the magnet. Step S40 is a step of performing a second heat treatment on the RTB system sintered magnet that has been subjected to the first heat treatment at a temperature of 450°C to 750°C and lower than the temperature of the first heat treatment in a vacuum or inert gas environment. The above steps are described in more detail below.
[0077] (Step of Preparing RTB-Based Sintered Body)
[0078] First, the composition of the RTB based sintered body will be described.
[0079] One of the characteristic points of the RTB system sintered body used in the present embodiment is that the RTB system sintered magnet that finally satisfies the above formula (1) is produced by adjusting the R, oxygen content, carbon content, etc. contained in the RTB system sintered body. Therefore, in the RTB system sintered body, it is preferred to prepare an RTB system sintered body that satisfies the relationship of 0.85 mass% ≤ [B] ≤ 0.94 mass%, 25.8 mass% ≤ ≤ ([Nd] + [Pr] + [Ce] + [La] + [Dy] + [Tb]) - 12 ([O] + [C]) ≤ 27.5 mass%, and 0.05 mass% ≤ [O] ≤ 0.30 mass%. In addition, it is preferred to prepare an RTB system sintered body that satisfies the relationship of 0.05 mass% ≤ [C] ≤ 0.18 mass%. By subjecting such an RTB system sintered body to the diffusion process described later, R, M, etc. will not diffuse excessively into the interior of the RTB system sintered body, and grain boundary diffusion can be greatly promoted.
[0080] The RTB-based sintered body prepared in this step has, for example, the following composition.
[0081] R: 26.6 mass % or more and 31.5 mass % or less, wherein R is at least one of the rare earth elements and must contain Nd,
[0082] B: 0.85 mass % or more and 0.94 mass % or less,
[0083] M: 0 mass % or more and 1.5 mass % or less, wherein M is at least one selected from Ga, Cu, Zn, Al and Si,
[0084] Q: 0 mass % or more and 2.0 mass % or less, wherein Q is at least one selected from Ti, V, CR1-Mn, Ni, Zr, Nb, Mo, Ag, In, Sn, Hf, Ta, W, Pb and Bi,
[0085] The remainder is T (T is Fe or Fe and Co) and inevitable impurities.
[0086] The RTB-based sintered body also satisfies the above formula (1).
[0087] Next, a method for preparing the RTB based sintered body will be described.
[0088] First, after preparing an alloy for RTB based sintered magnets, the alloy is coarsely pulverized by, for example, hydrogen pulverization.
[0089] The method for manufacturing an alloy for RTB-based sintered magnets is described below. The alloy ingot can be obtained by an ingot casting method in which a metal or alloy that has been adjusted to the above composition is melted and poured into a mold to solidify it. In addition, the alloy can also be prepared by a thin strip continuous casting method in which a quenched and solidified alloy is made by contacting a molten metal or alloy that has been adjusted to the above composition with a single roller, a double roller, a turntable or a rotating cylindrical mold, etc., and quenching (sudden cooling) is performed. In addition, flaky alloys can also be manufactured by other quenching methods such as centrifugal casting.
[0090] In an embodiment of the present invention, an alloy manufactured by either an ingot casting method or a quenching method can be used, and an alloy manufactured by a quenching method such as a thin strip continuous casting method is preferably used. The thickness of the alloy prepared by the quenching method is usually in the range of 0.03 mm to 1 mm, and is in the form of a sheet. The alloy melt solidifies from the surface in contact with the cooling roller (roller contact surface), and the crystal grows into a columnar shape along the thickness direction from the roller contact surface. Compared with the alloy (ingot alloy) prepared by the previous ingot casting method (mold casting method), the quenched alloy can be cooled in a short time, so the structure is finer, the crystal grain size is smaller, and the grain boundary area is larger. Since the R-rich phase diffuses on a large scale within the grain boundary, the dispersibility of the R-rich phase of the quenching method is excellent. For this reason, the hydrogen crushing method is used, and the grain boundary is easily broken. By hydrogen crushing the quenched alloy, the size of the hydrogen crushed powder (coarse crushed powder) can be made to be, for example, less than 1.0 mm. The coarse crushed powder obtained in this way can be crushed by, for example, a jet mill.
[0091] In this embodiment, the conditions for the pulverization are adjusted so that the oxygen content of the RTB-based sintered magnet finally obtained is within a specific range (0.05 mass % ≤ [O] ≤ 0.30 mass %). Jet mill pulverization is pulverization performed under an inactive atmosphere such as nitrogen. The pulverization can also be performed by jet mill pulverization in a humidified atmosphere, for example. It is preferred to make the powder particles smaller (the average particle size is greater than 2.0 μm and less than 10.0 μm, more preferably the average particle size is greater than 2.0 μm and less than 8.0 μm, further preferably the average particle size is greater than 2.0 μm and less than 4.5 μm, and further preferably the average particle size is greater than 2.0 μm and less than 3.5 μm). By making the powder particles smaller, a high H cJ .
[0092] As long as the above conditions are met, the fine powder used for preparing the RTB based sintered body may be prepared from one raw material alloy (single raw material alloy) or by using two or more raw material alloys and mixing them (blending method).
[0093] In a preferred embodiment, after a powder molded body is prepared from the above-mentioned fine powder by pressing in a magnetic field, the powder molded body is sintered. From the perspective of inhibiting oxidation, it is preferred that the pressing in a magnetic field adopts a method of forming a powder molded body by pressing in an inert gas environment or wet pressing. In particular, wet pressing makes the surface of the particles constituting the powder molded body covered with a dispersant such as an oil agent, thereby inhibiting contact with oxygen and water vapor in the atmosphere. Therefore, it is possible to prevent or inhibit the particles from being oxidized by the atmosphere before or after the pressing process or during the pressing process. Therefore, it is easy to control the oxygen content within a specified range. In the case of wet pressing in a magnetic field, a slurry in which a dispersion medium is mixed in the fine powder is prepared, provided to the mold cavity of the wet pressing device, and pressed in a magnetic field. It should be noted that the RTB-based sintered body can also be prepared without molding, etc., by using a known method such as the PLP (Press-Less Process: pressureless process) method described in Japanese Patent Laid-Open No. 2006-19521.
[0094] The molded body is then sintered to obtain an RTB-based sintered body. The sintering of the molded body is preferably carried out at a temperature range of 950°C to 1150°C. To prevent oxidation caused by sintering, the residual gas in the atmosphere can be replaced with an inactive gas such as helium or argon. The obtained sintered body can also be heat-treated. The heat treatment conditions such as the heat treatment temperature and heat treatment time can adopt known conditions.
[0095] (Process of preparing R1-M alloy)
[0096] In the present embodiment, an alloy containing R1 or R1 and M is diffused from the surface to the inside of the RTB based sintered body. Therefore, an R1-M alloy containing these elements to be diffused is prepared.
[0097] First, the composition of the R1-M alloy is described. R1 in the R1-M alloy is at least one of the rare earth elements. Preferably, R1 is more than 65% by mass and less than 100% by mass of the entire R1-M alloy, and M is at least one selected from Ga, Cu, Zn, Al, and Si, preferably more than 0% by mass and less than 35% by mass of the entire R1-M alloy. It is also preferred that R1 contains at least one of Nd and Pr, and more preferably R1 must contain Pr, and the Pr content in R1 is preferably more than 65% by mass and less than 86% by mass of the entire R1-M alloy. Preferably, the Pr content of the R1-M alloy accounts for more than 50% by mass of the entire R1, and more preferably, the Pr content of the R1-M alloy accounts for more than 65% by mass of the entire R1. Since the presence of Pr facilitates diffusion in the grain boundary phase, it can promote grain boundary diffusion and obtain higher H cJ .
[0098] The shape and size of the R1-M alloy are not particularly limited and are arbitrary. The R1-M alloy can be in the form of a film, foil, powder, block, granule, or the like.
[0099] Next, the method for preparing the R1-M alloy is described.
[0100] The R1-M alloy can be prepared by a raw material alloy preparation method used in a conventional RTB-based sintered magnet manufacturing method, such as a mold casting method, a thin strip continuous casting method, a single-roll ultrafast quenching method (melt spinning method), an atomization method, etc. In addition, the R1-M alloy can also be a product obtained by pulverizing the alloy obtained as described above by a known pulverization method such as a pin mill.
[0101] (Diffusion process)
[0102] At least a portion of the R1-M alloy is brought into contact with at least a portion of the surface of the RTB-based sintered body prepared by the above method, and a first heat treatment is performed at a temperature of 700°C to 950°C in a vacuum or inert gas environment, thereby performing a diffusion step of diffusing R1 and M into the interior of the magnet. Thus, a liquid phase containing R1 and M is generated from the R1-M alloy, and the liquid phase diffuses from the surface of the sintered body through the grain boundaries in the RTB-based sintered body and is introduced into the interior.
[0103] When the first heat treatment temperature is lower than 700°C, the amount of the liquid phase containing R1 and M will be too small, and high H cJ On the other hand, when the temperature exceeds 950℃, H cJIt is possible to reduce. It is preferably above 850°C and below 950°C. This can obtain a higher H cJ In addition, it is preferred that the RTB based sintered magnet subjected to the first heat treatment (700°C or higher and 950°C or lower) is cooled from the temperature at which the first heat treatment was performed to 300°C at a cooling rate of 5°C / min or higher. This can obtain a higher H cJ More preferably, the cooling rate to 300° C. is 15° C. / min or more.
[0104] The first heat treatment can be performed by configuring an R1-M alloy of any shape on the surface of the RTB system sintered body using a known heat treatment device. For example, the surface of the RTB system sintered body can be covered with a powder layer of the R1-M alloy and the first heat treatment can be performed. It is also possible to, for example, apply a slurry obtained by dispersing the R1-M alloy in a dispersion medium on the surface of the RTB system sintered body, evaporate the dispersion medium, and contact the R1-M alloy with the RTB system sintered body. It should be noted that as a dispersion medium, examples such as alcohols (ethanol, etc.), aldehydes and ketones can be cited. In addition, the R1-M alloy can also be formed into a film on the surface of the RTB system sintered body by, for example, a known sputtering device, and the first heat treatment can be performed. In addition, the introduction of the heavy rare earth element RH can be performed not only by the R1-M alloy, but also by configuring the fluoride, oxide, and oxyfluoride of the heavy rare earth element RH together with the R1-M alloy on the surface of the RTB system sintered magnet to introduce the heavy rare earth element RH. Examples of the fluoride, oxide, and oxyfluoride of the heavy rare earth element RH include TbF 3 , DyF 3 , Tb 2 O 3 , Dy 2 O 3 , TbOF, and DyOF.
[0105] The arrangement position of the R1-M alloy is not particularly limited as long as at least a portion of the R1-M alloy can be in contact with at least a portion of the RTB based sintered body.
[0106] (Step of Implementing Second Heat Treatment)
[0107] The RTB system sintered body subjected to the first heat treatment is heat treated in a vacuum or inert gas environment at a temperature of 400°C to 750°C and lower than the temperature of the first heat treatment step. In the present invention, this heat treatment is referred to as the second heat treatment. By performing the second heat treatment, a high H cJ When the temperature of the second heat treatment is higher than that of the first heat treatment, or the temperature of the second heat treatment is lower than 400°C or higher than 750°C, it may not be possible to obtain high H cJ .
[0108] Example
[0109] Example 1
[0110] The raw materials of each element were weighed so that the RTB-based sintered body had the composition shown in No. A to P in Table 1, and alloys were prepared by thin strip continuous casting. The obtained alloys were coarsely pulverized by hydrogen crushing to obtain coarse pulverized powder. Then, zinc stearate as a lubricant was added to the obtained coarse pulverized powder and mixed, and then dry pulverized in a nitrogen stream using an air flow pulverizer (jet mill device) to obtain a pulverized particle size D 50 The finely pulverized powder (alloy powder) is 3 μm in size. After zinc stearate as a lubricant is added and mixed into the above-mentioned finely pulverized powder, it is molded in a magnetic field to obtain a molded body. It should be noted that the molding device uses a so-called right-angle magnetic field molding device (transverse magnetic field molding device) in which the direction of magnetic field application is orthogonal to the direction of pressure application. The obtained molded body is fired in a vacuum at a temperature of more than 1000°C and less than 1090°C (each sample is selected to be a temperature sufficient to become dense by sintering) for 4 hours to obtain an RTB-based sintered body. The density of the obtained RTB-based sintered body is 7.5Mg / m 3 The composition results of the obtained RTB-based sintered body are shown in Table 1. In addition, each component in Table 1 was measured using high-frequency inductively coupled plasma optical emission spectrometry (ICP-OES).
[0111] [Table 1]
[0112]
[0113] The raw materials of each element were weighed so that the R1-M alloy had approximately the composition shown in No.a and No.b in Table 2, and these raw materials were melted and a strip or sheet alloy was obtained by a single roll ultrafast quenching method (melt spinning method). The obtained alloy was crushed in a mortar under an argon atmosphere and passed through a sieve with an aperture of 425 μm to prepare the R1-M alloy. The composition of the obtained R1-M alloy is shown in Table 2.
[0114] [Table 2]
[0115]
[0116] The RTB sintered bodies No. A to P in Table 1 are cut and ground to form cubes of 7.4 mm × 7.4 mm × 7.4 mm. Next, R1-M alloys (No. a and b) are spread over the entire surface of the R1-TB sintered bodies No. A to P in a range of 1.7 to 4.2 mass % relative to 100 mass % of the RTB sintered bodies. The RTB sintered magnet No. 1 shown in Table 3 is a product obtained by a diffusion process using the RTB sintered body No. B in Table 1 and the R1-M alloy No. a. The same is true for No. 2 to 16. The diffusion process is carried out in a reduced pressure argon gas controlled at 50 Pa, and the first heat treatment is performed at a temperature of 900°C for 4 hours and then cooled to room temperature. In this way, an RTB sintered magnet subjected to the first heat treatment is obtained. The RTB system sintered magnet that had undergone the first heat treatment was then subjected to a second heat treatment at 480°C for 3 hours in a reduced pressure argon atmosphere controlled at 50 Pa, and then cooled to room temperature to produce RTB system sintered magnets (No. 1 to 16). The composition of the resulting RTB system sintered magnet is shown in Table 3. Formula (2) is the value of ([Nd] + [Pr] + [Ce] + [La] + [Dy] + [Tb]) - 12 ([O] + [C]). It should be noted that the oxygen (O) content was measured using a gas analyzer using a gas fusion-infrared absorption method. It was also confirmed whether the atomic ratio of B to T in the RTB system sintered magnet was lower than R2T 14 The ratio of the number of atoms of B to T in the stoichiometric composition of the B compound. The results are shown in formula (1) in Table 3. When the relationship of [T] / 55.85>14×[B] / 10.8 is satisfied, it is marked as "○", and when it is not satisfied, it is marked as "×". The obtained RTB-based sintered magnet was machined to a sample of 7mm×7mm×7mm, and the magnetic properties were measured using a BH tracer. The measurement results are shown in Table 3. In addition, after line analysis (line analysis) was performed on the cross-section of the magnets No. 1 to 16 from the surface of the magnet to the vicinity of the center of the magnet using EDX, it was confirmed that the concentrations of Tb, Pr, Ga and Cu in No. 14 gradually decreased from the surface of the magnet to the center of the magnet (the concentration gradually decreased). It was also confirmed that the concentrations of Pr, Ga and Cu in the other magnets (No. 1 to 13, No. 15 and 16) gradually decreased from the surface of the magnet to the center of the magnet (the concentration gradually decreased).
[0117] [Table 3]
[0118]
[0119] As shown in Table 3, Examples No. 1 to 13 of the present invention do not contain Tb, and the residual magnetic flux density (B r) is above 1.40T, the coercive force (H cJ ) is above 1400kA / m, and when B r Set the value of (T) to [Y], H cJ When the value (kA / m) is set to [X], the relationship [Y]≥-0.0002×[X]+1.73 is satisfied, which can reduce the usage of heavy rare earth elements RH such as Tb and have high B r and high H cJ In contrast, the comparative examples (No. 15 and 16) that deviate from the scope of the present invention cannot achieve the residual magnetic flux density (B r )1.40T or more, coercive force (H cJ )High B above 1400kA / m r and high H cJ In Example No. 14 of the present invention, 0.05 mass % ≤ [Tb] ≤ 0.20 mass %, and the residual magnetic flux density (B r ) is 1.43T or more, and the coercive force (H cJ ) is above 1900kA / m, which reduces the usage of heavy rare earth elements RH such as Tb and has high B r and high H cJ RTB sintered magnet.
[0120] Explanation of symbols
[0121] 12: R2T included 14 Main phase of compound B
[0122] 14: Grain boundary phase
[0123] 14a: Two grain boundary phases
[0124] 14b: Grain boundary triple point
Claims
1. A RTB based sintered magnet, characterized in that: The RTB sintered magnet comprises: 14 B compound, and a grain boundary phase located at the grain boundary portion of the main phase, wherein R is at least one of the rare earth elements and must contain Nd, T is Fe or Fe and Co, and B is boron, When the Nd content (mass %) is [Nd], The content (mass %) of Pr is [Pr], The Ce content (mass %) is denoted as [Ce], The content (mass %) of La is [La], The content (mass %) of Dy is represented by [Dy], The content (mass %) of Tb is [Tb], The content (mass %) of B is [B], The content (mass %) of O is [O], The content (mass %) of C is [C], The content (mass %) of M is [M], where M is at least one selected from Ga, Cu, Zn, Al and Si, The atomic ratio of B to T in RTB sintered magnets is lower than that in R2T 14 The stoichiometric composition of the B-type compound is the ratio of the number of atoms of B to T, and satisfies 26.0 mass%≤([Nd]+[Pr]+[Ce]+[La]+[Dy]+[Tb])-12([O]+[C])≤27.7 mass%, 0.85 mass%≤[B]≤0.94 mass%, 0.05 mass%≤[O]≤0.30 mass%, 0.05 mass%≤[M]≤2.00 mass%, The relationship between [Tb]≤0.20 mass% and [Dy]≤0.30 mass%, The RTB based sintered magnet includes a portion in which at least one of a Nd concentration and a Pr concentration gradually decreases from a magnet surface toward an inner portion of the magnet.
2. The RTB based sintered magnet according to claim 1, characterized in that: It includes a portion where the M concentration gradually decreases as going from the surface of the magnet toward the inside of the magnet.
3. The RTB based sintered magnet according to claim 1 or 2, characterized in that: It includes a portion where the Pr concentration gradually decreases as going from the surface of the magnet toward the inside of the magnet.
4. The RTB based sintered magnet according to any one of claims 1 to 3, characterized in that: 0.85 mass%≤[B]≤0.92 mass%.
5. The RTB based sintered magnet according to any one of claims 1 to 4, characterized in that: 0.05 mass%≤[Tb]≤0.20 mass%, residual flux density (B r ) is above 1.43T, the coercive force (H cJ ) is above 1900kA / m.
6. The RTB based sintered magnet according to any one of claims 1 to 5, characterized in that: Does not contain Tb (except unavoidable impurities), residual flux density (B r ) is above 1.40T, the coercive force (H cJ ) is above 1400kA / m, and when B r Set the value of (T) to [Y], H cJ When the value (kA / m) is set to [X], the relationship [Y]≥-0.0002×[X]+1.73 is satisfied.
7. The RTB based sintered magnet according to any one of claims 1 to 6, characterized in that: The RTB based sintered magnet contains Ga and Cu. When the Ga content (mass %) is [Ga] and the Cu content (mass %) is [Cu], [Ga]≥1.2×[Cu].