MOF separation membrane, preparation method and application of MOF separation membrane in organic azeotropic system separation

By regulating the metal source and post-synthesis repair strategies, the lattice defects of the MOF-801 film are reduced, and the problem of insufficient separation performance of the existing MOF-801 film in the organic azeotropic system is solved, and efficient screening of molecules of different kinetic diameters is achieved. The thermal and chemical stability of the membrane is improved.

CN118904112AActive Publication Date: 2024-11-08NANJING TECH UNIV

Patent Information

Application Number
CN202310509317.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

The existing MOF-801 films have lattice defects in the separation of organic azeotropic systems, resulting in limited separation performance, especially poor separation performance with kinetic diameters greater than their intrinsic lattice pore size.

Method used

By regulating the metal source and post-synthesis repair strategy, the crystal defects of the film are reduced. The molar ratio of ZrCl4 to fumaric acid is 1:0.8 to 1.3, zirconium chloride is used as the metal source, and post-repair is performed to reduce lattice defects. A MOF-801 film layer with a pore size of 0.5-0.6 nm was formed.

Benefits of technology

It significantly improves the separation performance of MOF membrane in azeotropic systems such as methanol/dimethyl carbonate, methanol/methyl acetate, methanol/methyl tert-butyl ether, and realizes the precise regulation of intrinsic subnanometer mass transfer lattice pores. Enhanced thermal and chemical stability of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904112A_ABST
    Figure CN118904112A_ABST
Patent Text Reader

Abstract

The invention discloses an MOF (Metal Organic Framework) separation membrane, a preparation method and application of the MOF separation membrane in organic azeotropic system separation, and provides a modulation metal source type and a post-synthesis repair strategy for inhibiting lattice defects in an MOF-801 membrane aiming at the problem that the separation performance of the membrane is reduced due to lattice defects of the MOF-801 membrane prepared by an in-situ solvothermal method. Precise regulation and control of effective screening holes in the MOF-801 membrane are realized, so that intrinsic sub-nanometer mass transfer lattice holes in the membrane are constructed, and based on a size screening mechanism, the separation performance of the MOF membrane in azeotropic systems such as methanol / dimethyl carbonate, methanol / methyl acetate and methanol / methyl tert-butyl ether is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an MOF separation membrane, a preparation method and application thereof in organic azeotropic system separation, and belongs to the technical field of membrane separation. Background Art

[0002] In 2012, Behrens' research group first synthesized a new zirconium-based MOF, Zr-fumarate, by hydrothermal method. In 2014, Yaghi's research group officially named it MOF-801. MOF-801 is PN3 - Structure, Zr 4+ It has a tetragonal antiprismatic coordination geometry and has 8 oxygen atoms ( Figure 1 ). Its three-dimensional framework is constructed by ZrO2 secondary structural units. ZrO2 secondary structural units are composed of six crystallographically equivalent Zr 4+ Each secondary structural unit is coordinated and connected with 12 organic ligands (fumaric acid). Its three-dimensional skeleton is composed of a fumarate and two secondary structural units, forming porous tetrahedral and octahedral cages. This space group has two independent tetrahedral cavities with different sizes, with diameters of and The diameter of the octahedral cavity is Its minimum window size Just between methanol With most ester organic substances (such as dimethyl carbonate: ) between the kinetic diameters. In addition, based on the hard-soft acid-base theory, MOF-801 is composed of Zr 4+ The coordination bond strength between the carboxylic acid ligands is extremely high, which makes it have excellent water stability, thermal stability and chemical stability. Therefore, MOF-801 is expected to achieve efficient screening of liquid mixtures.

[0003] MOF-801 was used as the separation membrane research object, and the MOF-801 membrane was constructed by in-situ synthesis method (the membrane schematic diagram is shown in Figure 2 When the separation performance of the prepared MOF membrane for organic azeotropic systems was positively correlated with the kinetic diameter of the organic molecules, indicating that size screening was dominant. Moreover, the separation performance of the MOF-801 membrane for systems with kinetic diameters larger than its intrinsic lattice pore size was limited, indicating the presence of lattice defects in the membrane. Summary of the invention

[0004] The purpose of the present invention is to provide a MOF separation membrane, a preparation method and its application in the separation of organic azeotropic systems, and to reduce the crystal defects of the membrane by regulating the metal source and post-synthesis repair strategy, so that the membrane has excellent separation performance, thermal stability and chemical stability.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A MOF separation membrane comprises a support and a membrane layer, wherein the support is a porous material;

[0007] The membrane layer is composed of MOF-801, the membrane layer thickness is 1-5 μm, the pore size is 0.5-0.6 nm, and the specific surface area of ​​the membrane layer is 400-500 m 2 / g; characterized in that the lattice defects of MOF-801 in the film layer are less than 15%.

[0008] Preferably, the material of the support body is α-Al2O3, and the support body is a porous structure with a pore size of 100-300nm and a porosity of 20%-45%.

[0009] The method for preparing the above MOF separation membrane comprises the following steps:

[0010] Film casting: fix the support in the reactor, pour in the casting solution to make the film, cool it down after completion, exchange the solvent of the sample, and then dry it to obtain the MOF separation membrane;

[0011] The casting solution is a mixed solution of an organic solvent and formic acid dissolved with ZrCl4 and fumaric acid, and in the casting solution, the molar ratio of ZrCl4 to fumaric acid is 1:0.8-1.3; the volume ratio between the organic solvent and formic acid is 100:20-50.

[0012] Preferably, it also includes a post-repair step, which is to fix the membrane in a reactor after obtaining the separation membrane, pour a repair solution into it for post-repair, cool it after completion, perform solvent exchange on the sample, and then dry it to obtain a post-repaired MOF separation membrane;

[0013] The repair liquid is a mixed solution of an organic solvent in which fumaric acid is dissolved and formic acid; the volume ratio between the organic solvent and formic acid is 100:20-50.

[0014] Preferably, the support body has a thickness of 1-5 mm and a diameter of 20-40 mm.

[0015] Preferably, in the film casting step, the film is prepared by drying at 65-100° C. for 8-15 hours.

[0016] Preferably, in the post-repair step, the repair is specifically: drying at 70-90° C. for 9-14 hours.

[0017] Preferably, the lattice defects of MOF-801 in the MOF separation membrane layer obtained by post-repair are less than 6%.

[0018] Application of the above MOF separation membrane in the separation of organic azeotropic systems.

[0019] Preferably, the organic azeotropic system refers to an azeotropic system such as alcohol / dimethyl carbonate, methanol / methyl acetate, methanol / methyl tert-butyl ether, etc.

[0020] The beneficial effects of the present invention are:

[0021] In order to solve the problem that lattice defects in MOF-801 membrane prepared by in situ solvothermal method reduce the membrane separation performance, a strategy of adjusting the metal source type and post-synthesis repair is proposed to inhibit the lattice defects in the MOF-801 membrane, thereby achieving precise control of the effective screening pores in the MOF-801 membrane, thereby constructing intrinsic sub-nanometer mass transfer lattice pores in the membrane. Based on the size screening mechanism, the separation performance of MOF membrane in azeotropic systems such as methanol / dimethyl carbonate, methanol / methyl acetate, and methanol / methyl tert-butyl ether is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the structure of MOF-801;

[0023] Figure 2 Schematic diagram of MOF-801 membrane;

[0024] Figure 3 It is a schematic diagram of a pervaporation membrane device;

[0025] Figure 4 α-Al2O3 support body SEM images, wherein (A) is a SEM surface photo of the α-Al2O3 support body; (B) is a SEM cross-sectional photo of the α-Al2O3 support body;

[0026] Figure 5 SEM photos of MOF-801 membranes at different membrane preparation temperatures;

[0027] Figure 6 The SEM photos of MOF-801 membranes at different film preparation times at 80°C;

[0028] Figure 7 (A) XRD spectrum of MOF-801 film prepared on α-Al2O3 support using in-situ synthesis method; (B) Fourier transform infrared spectrum; (C) TG spectrum; (D) BET spectrum;

[0029] Figure 8 The effect of membrane temperature and membrane time on the separation performance of methanol / DMC by pervaporation of MOF-801 membrane;

[0030] Fig. 9 This is the pervaporation separation performance diagram of MOF-801 membrane for three organic-organic systems;

[0031] Fig.10The gas separation performance of MOF-801 membrane;

[0032] Fig.11 The SEM images of MOF-801 membranes with different film preparation times using zirconium chloride as the metal source;

[0033] Fig.12 The effect of membrane preparation time on the performance of MOF-801 membrane pervaporation separation of methanol / DMC using zirconium chloride as a metal source;

[0034] Fig.13 The pervaporation performance of MOF-801 membrane using zirconium chloride as metal source for three organic-organic systems;

[0035] Fig.14 SEM photos of MOF-801 membranes at different repair times;

[0036] Fig.15 The methanol / dimethyl carbonate pervaporation separation performance diagram of MOF-801 membrane with different repair time;

[0037] Fig.16 The pervaporation separation performance diagram of three organic-organic systems of post-repaired MOF-801 membrane;

[0038] Fig.17 (A) NMR defect concentration diagram of three different MOF-801 membranes; (B) PXRD spectrum; (C) N2 adsorption amount; (D) specific surface area and pore size diagram. DETAILED DESCRIPTION

[0039] The present invention will be specifically described below in conjunction with the accompanying drawings and embodiments.

[0040] Comparative Example 1

[0041] Preparation of alumina support

[0042] A certain amount of α-Al2O3 powder was extruded into discs at 20MPa. The prepared α-Al2O3 support had a pore size of about 200nm and a porosity of 35%. The sintered α-Al2O3 had a thickness of 2mm and a diameter of 28mm. Before growing the MOF-801 membrane, the alumina surface was first polished with 800-grit sandpaper, then polished with 2000-grit sandpaper, rinsed with deionized water, and dried at 120°C for 24 hours.

[0043] Preparation of MOF-801 membrane

[0044] First, the homemade α-Al2O3 support was fixed in the reactor lining. The equimolar ratio of zirconium oxychloride octahydrate and fumaric acid were fully dissolved in a mixed solvent of DMF / formic acid to prepare a synthetic solution, and then the fully dissolved reaction film casting solution was slowly poured into the reactor lining, the reactor lining was sealed and placed in a metal reactor, and it was placed in an oven for coordination reaction. After the reaction was completed, the reactor was cooled to room temperature, the sample was taken out for solvent exchange, and finally the membrane was placed in a vacuum drying oven at 150°C for 12 hours.

[0045] Main analytical test methods

[0046] Basic characterization of samples

[0047] The thermal stability of MOF-801 film was studied by thermogravimetric analysis (TGA, NETZSCH, STA, 449F3), the heating atmosphere was nitrogen, and the heating rate was 10 ° C / min. The structural characteristics of MOF-801 film were characterized by X-ray diffraction (XRD, Rigaku, Miniflex600, Japan), and the scanning speed was 10 ° / min. The cross-section and surface morphology of MOF-801 film were observed by field emission scanning electron microscopy (FESEM, Hitachi Limited, S-4800, Japan), and the sample was gold-sprayed under vacuum conditions using an ion sputtering instrument (Hitachi, MC1000, Japan), and the gold-spraying time was 120 seconds. The chemical properties of MOF-801 film were analyzed by Fourier Transform Infrared Spectroscopy (FTIR, AVATAR-FT-IR-360, Thermoncolet, USA).

[0048] Gas separation test

[0049] In the laboratory, the separation performance of the membrane is evaluated by the constant pressure-variable volume method in the single-component gas test. The single-component gas permeation test is carried out at 0.2MPa and 25°C. When the system reaches a steady state, the gas permeation rate P is the average of more than three test results, and the calculation formula is as follows:

[0050]

[0051] Where P represents the gas permeation rate (1GPU = 10 -6 cm 3 (STP)cm -2 s -1 cmHg -1), Patm represents atmospheric pressure (atm), Δp and T represent transmembrane pressure difference (atm) and test temperature (℃), A is the effective area of ​​the membrane, and dV / dt corresponds to the volume displacement rate in the bubble flowmeter. The ideal selectivity of H2 / CO2 is calculated from the ratio of the permeation rates of pure gases and can be expressed as follows:

[0052]

[0053] Pervaporation test

[0054] The prepared MOF-801 membrane was assembled into a homemade assembly. Figure 3 This is a schematic diagram of the pervaporation device. The raw material liquid circulates between the raw material tank and the membrane assembly at a certain flow rate through a circulation pump, and the raw material liquid is at a temperature to be tested. Its concentration is generally expressed as the mass ratio of small molecular components (such as 10wt% methanol). The permeate vapor that passes through the membrane layer is condensed with liquid nitrogen and collected by a cold trap. After the vapor is liquefied, a gas chromatograph (GC-2014, Shimadzu, Japan) is used to measure the concentration on the raw material side and the permeate side. The pervaporation performance of the membrane is judged based on the total flux J and the separation factor β. The feed liquid is selected as a methanol / DMC solution, a methanol / MTBE solution and a methanol / MAC solution with a methanol content of 10wt%. Total flux J (kg·m -2 ·h -1 ) is calculated by the sample mass collected in the cold trap and the test time:

[0055]

[0056] Where W represents the total mass of the collected sample (kg), t and A represent the test time (h) and effective membrane area (m 2 ).

[0057] The separation factor is calculated using the following formula:

[0058]

[0059] Where X and Y represent the mass fractions of the components on the permeate side and the feed side, respectively.

[0060] Membrane micromorphology

[0061] Field emission scanning electron microscopy (SEM) of the homemade α-Al2O3 support Figure 4 From the electron microscope photos of the support surface and cross section, it can be judged that the surface of the α-Al2O3 ceramic sheet is smooth, suitable for film growth, and its pore size is about 200nm.

[0062] In order to explore the optimal preparation conditions of MOF-801 membrane, the effects of different temperatures and different membrane preparation times on membrane formation were investigated. Figure 5 The electron microscope photos of MOF-801 membranes with different film-forming temperatures and a film-forming time of 6 hours can be seen from the electron microscope photos. At 60℃ and 70℃, a continuous film cannot be formed, and the film layer is basically invisible on the cross section. This is because the temperature is too low and there is not enough energy supply. The MOF grains cannot nucleate on the α-Al2O3 support, and then cannot grow alternately to form a dense film layer. At 80℃ and 90℃, a continuous and dense film layer can be formed. From the cross section, the thickness of the film is about 1.5μm, but it can be clearly seen that there are cracks on the surface of the film prepared at 90℃. We believe that this is caused by the mismatch of the thermal expansion coefficients of the α-Al2O3 support and the MOF-801 membrane. At 100℃ and 110℃, due to the high temperature, the MOF-801 grains preferentially nucleate in the mother liquid rather than on the surface of the support, and only particles accumulate on the α-Al2O3 support. Therefore, the optimal temperature we chose is 80℃.

[0063] Then, the effect of synthesis time on the preparation of MOF-801 membrane was investigated at a synthesis temperature of 80°C. Figure 6 As shown in the figure, when the synthesis time is less than 6h, a large number of MOF particles accumulate on the surface of the support and no inter-growth film layer is formed. This is because the reaction time is short and the formed MOF particles are small, making it difficult for them to interact with each other to form a continuous film layer. When the synthesis time is extended to 6h, the surface of the α-Al2O3 support is completely covered by MOF particles and the crystals have a good inter-growth morphology. The film thickness is about 1.5μm. We further extended the synthesis time, and the surface morphology and film thickness of the prepared film remained basically unchanged, so the optimal film-making time is 6h.

[0064] Characterization of the physicochemical properties of membranes

[0065] The structural properties of MOF-801 membranes prepared on α-Al2O3 supports were investigated using XRD. Figure 7 A area). The prepared MOF-801 film shows the characteristic peak of MOF-801 crystal at about 10°, which is consistent with the standard spectrum of MOF-801. The characteristic peak of α-Al2O3 support appears at about 25° and 35°. The intensity of MOF-801 characteristic peak is weak, which may be due to the thin MOF film layer. Then we used FTIR to study the chemical properties of MOF-801 film, such as Figure 7 As shown in area B, at 3217 cm -1 The characteristic peak generated at 1655 cm is the -OH bond of the Zr cluster. -1 The peak at 1580 cm is the -C=O bond in the solvent DMF. -1 , 1398cm -1 and 1207cm -1and 1103cm -1 The peaks are -C=O-OH and -C=O bonds generated by the functional groups of the organic ligand fumaric acid.

[0066] The thermal stability of MOF-801 membrane was investigated by TGA ( Figure 7 C area). The results show that before 100°C, the first slight weight loss of the MOF-801 sample was due to the removal of water absorbed by MOF-801. The second weight loss occurred at 100°C-260°C, which was due to the removal of guest molecules (such as methanol, N,N-dimethylformamide, etc.) in the pores of MOF-801. As the temperature increased further, at 260°C-500°C, the carboxylate groups decomposed successively, leading to the final decomposition of MOF-801. The above results show that the structural collapse temperature of MOF-801 is about 450°C, and the TGA results show that MOF-801 has better thermal stability than other MOF materials (about 350°C). N2 adsorption measurements at 77K show ( Figure 7 MOF-801 exhibits type I adsorption behavior, and the calculated BET surface area of ​​MOF-801 is 483.83 m 2 / g. The above results prove the successful preparation of MOF-801 membrane.

[0067] Organic azeotropic system performance test

[0068] The pervaporation experiment of methanol / dimethyl carbonate mixture (10 / 90wt%) was carried out at 50℃ to investigate the separation performance of MOF-801 membrane for organic azeotropes. Firstly, the effect of membrane preparation temperature on the pervaporation separation performance of MOF-801 membrane was investigated. Figure 8 As shown in area A, when the synthesis temperature is less than 80 °C and greater than 90 °C, no continuous MOF membrane layer is formed on the surface of the porous support ( Figure 5 ), the permeation flux of the prepared MOF-801 membrane is as high as 30 kg·m -2 ·h -1 The methanol content on the permeate side was similar to that on the feedstock side, and no separation performance was shown. When the synthesis temperature was 80°C, an inter-grown MOF membrane layer was formed, which significantly improved the methanol / dimethyl carbonate separation performance (flux: 7.2 kg·m -2 ·h -1 , separation factor: 135, feed temperature: 50°C, feed concentration: 10wt% methanol). We then investigated the effect of membrane synthesis time on the separation performance of methanol / dimethyl carbonate ( Figure 8 Area B). As the synthesis time gradually increases, the permeation flux shows a downward trend, while the separation factor of methanol / dimethyl carbonate gradually increases. When the synthesis time is 2 to 4 hours, the permeation flux of the membrane reaches 150 kg·m -2·h -1 , the separation factor of methanol / dimethyl carbonate is only about 3. This is because the continuous membrane layer does not completely cover the surface of the porous support, and there are a large number of macroporous defects (such as Figure 6 When the synthesis time was extended to 6 h, the permeation flux of methanol / dimethyl carbonate decreased to 7.5 kg·m -2 ·h -1 , the separation factor increased to 130, and then the separation factor and permeate flux tended to be stable when the synthesis time was extended. This shows that when the synthesis time was greater than 6h, the MOF-801 membrane with a mass transfer channel with molecular sieving effect had been formed, which can also be verified by SEM characterization ( Figure 6 ).

[0069] In order to further study the molecular sieving ability of MOF-801 membrane, we also investigated the separation performance of the prepared MOF membrane for two other organic azeotropic systems with different kinetic diameters, methanol / methyl tert-butyl ether and methanol / methyl acetate like Fig. 9 As shown in Figure 2, for the methanol / methyl acetate system, the MOF-801 membrane exhibited a high permeation flux of 8.9 kg·m -2 ·h -1 The separation factor was as low as 72. Meanwhile, for the methanol / dimethyl carbonate system, the permeation flux was reduced to 7.8 kg·m -2 ·h -1 , the separation factor is improved. This may be due to the larger kinetic diameter of dimethyl carbonate, which will hinder the diffusion of methanol to a certain extent. Interestingly, further increasing the kinetic diameter of organic molecules to When the separation factor of the MOF membrane increases to 200, it shows a certain separation performance. This is because the methanol molecule has a smaller kinetic diameter They can quickly pass through the MOF membrane pores, while ester or ether molecules have a larger dynamic diameter and will encounter greater mass transfer resistance when passing through the MOF membrane pores, thereby achieving effective screening of the two, indicating that the size screening mechanism is dominant.

[0070] According to literature reports, the sieve pore diameter of MOF-801 is about It is just between the kinetic diameter of methanol With dimethyl carbonate Methyl tert-butyl ether The kinetic diameter of the MOF-801 membrane is based on size screening. In theory, the MOF-801 membrane can achieve efficient screening of methanol / dimethyl carbonate and methanol / methyl tert-butyl ether. However, the separation factor of the MOF-801 membrane prepared by in situ hydrothermal treatment is only 72 to 130 for the two systems. We speculate that there may be lattice defects (cluster loss or ligand loss) in the prepared MOF-801 membrane, which increases its screening pore size and thus reduces the molecular screening ability. In order to verify our conjecture, we used H2 / CO2 separation performance to evaluate the regularity of the membrane. Three MOF-801 membranes (M1, M2 and M3) were selected, as shown in Figure 2. Fig.10 As shown in the figure, the membrane prepared under the optimal conditions exhibits a high H2 permeability coefficient (8500GPU) and a H2 / CO2 selectivity of about 5, which is close to its Knudsen diffusion selectivity. Since the unit cell size of MOF-801 is 2nm, when gas molecules move in the membrane pores, the minimum pore size corresponding to Knudsen diffusion is 2nm, so the gas separation performance confirms the existence of lattice defects in the prepared MOF-801 membrane.

[0071] Example 1

[0072] Preparation of MOF-801 membrane by regulating metal sources

[0073] In this embodiment, the metal source we selected is ZrCl4, and the specific film making process is as follows: fix the homemade α-Al2O3 support to the bottom of the reactor lining, dissolve different masses of ZrCl4 and fumaric acid in a mixed solvent of DMF / formic acid (200mL / 70mL) to prepare a casting solution. Then slowly pour a certain amount of the synthetic solution into the reactor lining and place the lining in the metal reactor, and place the reactor in an oven for coordination reaction. After the reaction is completed, cool to room temperature, take out the sample, and then perform solvent exchange, and finally dry it at 150°C for 12 hours under vacuum.

[0074] Example 2

[0075] Preparation of MOF-801 membrane by post-repair strategy

[0076] The MOF-801 membrane prepared using ZrCl4 as the metal source was fixed at the bottom of the reactor, and the fumaric acid ligand was dissolved in a mixed solvent of DMF / formic acid (200mL / 70mL) to prepare a repair solution. The repair solution was then slowly poured into the reactor, which was sealed and placed in an oven to react for a certain period of time. After the reaction was completed, it was cooled to room temperature, the sample was taken out for solvent exchange, and finally dried in a vacuum drying oven at 150°C for 12 hours.

[0077] Calculation of defect concentration using NMR method

[0078] During the synthesis of MOF crystals, the regulator (mainly the monoacid) can coordinate with the metal clusters, resulting in the generation of ligand loss defects. Therefore, the content of the regulator can be used to quantify the concentration of lattice defects. 1 Based on HNMR data, the molar ratio between the modulator and the ligand can be calculated according to the following formula:

[0079]

[0080] Where N HMod and N Hlinker The NMR signals of the modulator and ligand are 1 H proton number. For example, for the ligand fumaric acid, Nbdc = 4. Mod.1H Int. and linker 1H Int. refer to the intensities of the modulator and ligand NMR signals, respectively.

[0081] Therefore, the lattice defect concentration (Cdef.) obtained from NMR data can be calculated by the following formula:

[0082]

[0083] In Comparative Example 1, the metal source used to prepare the MOF-801 membrane is zirconium oxychloride. Due to its low Zr-O bond energy, it is easy to react and the reaction rate is very fast, resulting in too fast nucleation of MOF-801 grains. During the nucleation process, a large number of lattice defects will be generated. In order to reduce the density of lattice defects in the membrane, zirconium chloride with higher bond energy is selected as the metal source. The bond energy of the Zr-Cl bond is higher than that of the Zr-O bond, so its reaction rate is also slowed down. As the nucleation rate slows down, the defects of the prepared MOF-801 membrane are reduced, and it is expected to show higher molecular sieving performance. At 80°C, the effect of synthesis time on the preparation of membranes using ZrCl4 as a metal source was systematically investigated. Fig.11 As shown in the figure, the time required to synthesize a continuous and dense film layer using zirconium chloride as a metal source is 12 hours, which is longer than the time (6 hours) when ZrOCl2 is used as a metal source. This is because in the MOF synthesis process, ZrCl4 must first be hydrolyzed into ZrOCl2 and then form metal clusters and then coordinate with organic ligands. Therefore, ZrCl4 has a lower reaction rate, which may produce a lower lattice defect concentration, and can achieve the improvement of the separation performance of the organic azeotropic system. Subsequently, the film making time was further extended, and the morphology of the film did not change significantly.

[0084] The MOF-801 membrane prepared using zirconium chloride as the metal source was subjected to pervaporation testing. The pervaporation performance test of methanol / dimethyl carbonate was also conducted at a test temperature of 50°C and a raw material liquid methanol / dimethyl carbonate mass ratio of 1 / 9. Fig.12As shown in Figure 2, due to the use of zirconium chloride as the metal source, the nucleation rate slowed down, the membrane defects decreased, and the separation factor increased to about 250, while the corresponding flux decreased to 5 kg·m -2 ·h -1 The effect of membrane preparation time on performance matches the electron microscope. The membrane performance reaches the best at 12 hours of membrane preparation time. Even if the membrane preparation time is further extended, the performance changes almost nothing. The pervaporation performance test and electron microscope photos show that the optimal conditions for preparing MOF-801 membrane using zirconium chloride as a metal source are 80°C and 12 hours.

[0085] The pervaporation separation performance of the MOF-801 membrane prepared using zirconium chloride as the metal source for three different organic-organic systems was then tested. The results showed that due to the reduction of defects, the separation factors of the three systems were improved compared to the MOF-801 membrane using zirconium oxychloride, while the flux decreased accordingly. Fig.13 As shown in Figure 2, for methanol / methyl tert-butyl ether, the separation factor reached 300 and the flux was 7 kg·m -2 ·h -1 , the methanol / dimethyl carbonate system is about 250, and the flux is 5.5 kg·m -2 ·h -1 After the metal source ligand was replaced, the nucleation rate of MOF-801 crystals slowed down, and the defects in the entire film formation process were reduced compared with the previous use of zirconium oxychloride as the metal source ligand, resulting in a certain degree of improvement in the separation performance of the MOF-801 membrane using zirconium chloride as the metal source for three different organic azeotropic systems. From the perspective of performance, it is more intuitive to see that the regulation of the defects of the MOF-801 membrane leads to an improvement in the membrane separation performance.

[0086] Although the defects of the MOF-801 membrane prepared using zirconium chloride as the metal source are significantly reduced compared to the MOF-801 membrane prepared using zirconium oxychloride as the metal source, and the pervaporation separation performance of the organic azeotropic system is also greatly improved, the in situ synthesis method itself is prone to defects in the prepared membrane. The nucleation and growth processes of the crystals in this method are carried out simultaneously, and a certain amount of defects will inevitably be generated in the film formation process. Therefore, we further regulate the MOF-801 membrane through post-repair means to reduce its defects and thus achieve its optimal separation performance for pervaporation separation of organic-organic mixtures.

[0087] Post-synthesis repair

[0088] The defects of MOF-801 membrane prepared using zirconium chloride as the metal source are reduced compared to those of MOF-801 membrane prepared using zirconium oxychloride as the metal source. However, defects are still inevitable during the membrane making process, so we perform post-synthesis repair on the membrane to further reduce its defects.

[0089] The specific method is to immerse the MOF-801 membrane prepared using zirconium chloride as the metal source in an organic ligand solution, and then put the membrane into an oven at 80°C for repair. Fig.14 It can be observed that the surface of the repaired membrane is smoother, but its thickness has not changed. And as the repair time increases, the membrane thickness has not changed significantly. However, it cannot be directly observed from the SEM photos, so other subsequent characterization tests and pervaporation performance tests are carried out.

[0090] The repaired MOF-801 membrane was then subjected to a pervaporation test. The pervaporation performance test of methanol / dimethyl carbonate was also conducted at a test temperature of 50°C and a raw material liquid methanol / dimethyl carbonate mass ratio of 1 / 9. Fig.15 From the above, the separation performance of the membrane repaired for 6 hours has not yet reached the optimal level, and its separation factor is only slightly improved compared with the unrepaired MOF-801 membrane prepared using zirconium chloride as the metal source. When the repair time is extended to 12 hours, the separation factor of the membrane reaches the optimal level. For the methanol / dimethyl carbonate system, the separation factor reaches about 350, and the flux is 4 kg·m -2 ·h -1 (Feed temperature: 50°C, feed concentration: 10 wt% methanol).

[0091] Compared with the MOF-801 membrane prepared using zirconium oxychloride (methanol / DMC system flux: 7.2 kg·m -2 ·h -1 , separation factor: 135, feed temperature: 50 °C, feed concentration: 10 wt% methanol) and unrepaired MOF-801 membrane prepared with zirconium chloride (methanol / DMC system, flux: 5.5 kg·m -2 ·h -1 , separation factor: 250, feed temperature: 50℃, feed concentration: 10wt% methanol), we have gradually reduced the membrane defects through a step-by-step strategy, and thus significantly improved its separation factor, while the flux has decreased accordingly. When the repair time continues to be extended, the performance of the membrane has no obvious change, indicating that the repair time of 12 hours is the best. When the repair reaches a certain limit, the extension time no longer plays a role in repairing defects.

[0092] For the MOF-801 membrane with a repair time of 12 h, we conducted pervaporation performance tests in three organic-organic systems, such as Fig.16 For methanol / methyl tert-butyl ether, the separation factor reached 520 and the flux was 3.8 kg·m -2 ·h -1 , the methanol / dimethyl carbonate system is about 350, and the flux is 3.7 kg·m-2 ·h -1 The separation factor of the methanol / methyl acetate system also reached about 220, and the flux was about 3.8 kg·m -2 ·h -1 .

[0093] Defect Characterization

[0094] First, we studied the lattice defects (ligand missing) of the three MOF-801 films by NMR. The lattice defect concentration can be obtained based on the peak area ratio of formic acid to ligand fumaric acid. Fig.17 As shown in area A, the MOF-801 membrane prepared using ZrOCl2 as the metal source has the most lattice defects, with a defect concentration of 19%. The lattice defect concentration of the membrane prepared by changing the metal source to ZrCl4 is reduced to 13.5%. This is because during the membrane making process, ZrCl4 needs to be hydrolyzed to form ZrOCl2 first, and then form metal clusters to coordinate with organic ligands. The reaction rate is significantly reduced, thereby reducing the defect concentration. After soaking in the ligand solution, its lattice defect concentration is further reduced (5%). The lattice defects of the MOF membrane include ligand missing defects and cluster missing defects. We also used PXRD to characterize and study the cluster missing defects of the MOF membrane. The changes in the cluster missing defects in the MOF membrane can be reflected by observing the intensity changes of the characteristic peaks of the cluster missing defects at around 5°. As shown Fig.17 As shown in area B, with the regulation of metal sources and the implementation of post-repair strategies, cluster missing defects gradually decrease, which is consistent with the change law of ligand missing defects. In addition, the reduction of lattice defects will cause the pore size of the MOF membrane to gradually approach the intrinsic pores of the MOF material, resulting in a reduction in surface area and adsorption sites. Therefore, the reduction of lattice defects can also be confirmed by gas adsorption and changes in specific surface area and pore size ( Fig.17 C area, D area), the above results confirm that the metal source regulation and post-repair strategy we proposed can effectively reduce the lattice defect concentration, thereby regulating the pore structure of the MOF membrane and achieving efficient screening of molecules.

[0095] The above is only a preferred implementation of the patent of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the patent of the present invention. These improvements and modifications should also be regarded as the protection scope of the patent of the present invention.

Claims

1. A MOF separation membrane, comprising a support and a membrane layer, wherein the support is a porous material; The membrane layer is composed of MOF-801, the membrane layer thickness is 1-5 μm, the pore size is 0.5-0.6 nm, and the specific surface area of ​​the membrane layer is 400-500 m 2 / g; characterized in that The lattice defect of MOF-801 in the film layer is less than 15%.

2. The MOF separation membrane according to claim 1, characterized in that The material of the support body is α-Al2O3, and the support body is a porous structure with a pore size of 100-300nm and a porosity of 20%-45%.

3. The method for preparing the MOF separation membrane according to any one of claims 1 to 2, characterized in that: The steps include: Film casting: fix the support in the reactor, pour in the casting solution to make the film, cool it down after completion, exchange the solvent of the sample, and then dry it to obtain the MOF separation membrane; The casting solution is a mixed solution of an organic solvent and formic acid dissolved with ZrCl4 and fumaric acid, and in the casting solution, the molar ratio of ZrCl4 to fumaric acid is 1:0.8-1.3; the volume ratio between the organic solvent and formic acid is 100:20-50.

4. The method for preparing a MOF separation membrane according to claim 3, characterized in that: The method also includes a post-repair step, which is to fix the membrane in a reactor after obtaining the separation membrane, pour a repair solution into the reactor for post-repair, cool the sample after completion, perform solvent exchange on the sample, and then dry the sample to obtain a post-repaired MOF separation membrane. The repair liquid is a mixed solution of an organic solvent in which fumaric acid is dissolved and formic acid; the volume ratio between the organic solvent and formic acid is 100:20-50.

5. The method for preparing a MOF separation membrane according to claim 3, characterized in that: The support body has a thickness of 1-5 mm and a diameter of 20-40 mm.

6. The method for preparing a MOF separation membrane according to claim 3, characterized in that: In the film casting step, the film is prepared by drying at 65-100° C. for 8-15 hours.

7. The method for preparing a MOF separation membrane according to claim 4, characterized in that: In the post-repair step, the repair is specifically: drying at 70-90°C for 9-14 hours.

8. The method for preparing a MOF separation membrane according to claim 4, characterized in that: The lattice defect of MOF-801 in the MOF separation membrane layer obtained after repair is less than 6%.

9. Use of the MOF separation membrane according to any one of claims 1 to 2 in separation of an organic azeotropic system.

10. The use according to claim 9, characterized in that: The organic azeotropic system refers to the alcohol / dimethyl carbonate, methanol / methyl acetate, and methanol / methyl tert-butyl ether azeotropic systems.

Citation Information

Patent Citations

  • Method for preparing defect-free MOF-801 film by small seed crystal induced film formation-surfactant post-modification strategy and application thereof

    CN111054223A

  • Preparation method of small-size MOF-801 material

    CN113801334A

  • Method for improving preparation of Zr-based MOF (Metal Organic Framework) membrane by using intermediate modification layer and forward osmosis application of Zr-based MOF membrane

    CN114471200A

  • Method for predicting lattice defects of MOF (Metal Organic Framework) film

    CN115831286A

  • Metal-organic framework

    GB202110269D0

Cited By

  • Preparation method of novel Zr-MOF membrane and organic matter separation application

    CN120532315A

  • Two-dimensional layered membrane for nanofiltration separation as well as preparation method and application of two-dimensional layered membrane

    CN121490570A