Pelletizing method of catalyst for synthesizing carbon nanotube fibers

The catalyst component powder is made into spherical particles through wet granulation method, which solves the problem of existing catalysts being stratified and absorbed in high-temperature reaction equipment, improves the uniformity and stability of the catalyst, and significantly improves the carbon nanotubes Product quality and catalytic properties of fibers.

CN118904362APending Publication Date: 2024-11-08WUXI DONGHENG NEW ENERGY TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411038207.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing catalysts used to synthesize carbon nanotube fibers have different layers of precipitation and moisture absorption and oxidation in high-temperature plasma reaction equipment, and their catalytic performance is lower than the theoretical level.

Method used

By using wet granulation method, the powder of each component of the catalyst is prepared into spherical particles, and bonded them together through binders and wetting agents to form spherical particles, improving fluidity and stability, and preventing component segregation and moisture absorption. .

Benefits of technology

It improves the uniformity and stability of the catalyst, enhances the catalytic performance, ensures the activity and service life of the catalyst, and reduces the powder resistance and ash content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904362A_ABST
    Figure CN118904362A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of catalysts, and provides a granulation method of a catalyst for synthesizing carbon nanotube fibers, which comprises the following steps: fully mixing raw material powder according to a formula to obtain mixed powder; the method comprises the following steps: uniformly mixing a binder and a wetting agent to prepare a binder solution with the concentration of 0.5-6wt%; the decomposition temperature of the binder is 200-300 DEG C; the wetting agent is volatile liquid; the mixed powder and the binder solution are prepared into spherical particles of 20-30 meshes through wet granulation; and drying to obtain the catalyst for synthesizing the carbon nanotube fiber. Wherein the weight ratio of the mixed powder to the binder is 100: (0.05-1), and the prepared catalyst for synthesizing the carbon nanotube fibers is high in particle strength and has excellent catalytic activity, the IG / ID is remarkably improved compared with that of ungranulated catalyst powder, the IG / ID is up to 120 at most, the ash content is relatively low, and the minimum powder resistance is less than 15 m omega.cm <-1 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a granulation method of a catalyst for synthesizing carbon nanotube fibers, and belongs to the technical field of catalyst chemical engineering. Background Art

[0002] Since carbon nanotubes were first synthesized, they have attracted great attention in the fields of materials science and physics. Carbon nanotubes present a nanoscale tubular structure, which gives them unique electronic, mechanical and chemical properties and has a wide range of application potential. Carbon nanotube fibers are a special form of carbon nanotubes. The production technology of carbon nanotubes is mainly divided into chemical vapor deposition, arc discharge, laser evaporation and flame deposition. Among them, chemical vapor deposition is the most mainstream production technology, accounting for more than 90% of carbon nanotube production, with high yield, low cost and good controllability.

[0003] The preparation process of carbon nanotube fibers usually uses a high-temperature plasma reaction device (plasma high-temperature furnace). The inventors have found through long-term research that the existing catalysts have inconsistent densities of various components. When they are fed into the high-temperature zone of the high-temperature plasma reaction device through a vibrating feeding device, the various components of the catalyst are separated into layers due to vibration and other reasons, resulting in uneven catalyst components entering the high-temperature zone, which is not conducive to its catalytic performance; the particle size of various components of the existing catalyst is usually 5 to 10 μm, and its specific surface area is large, which makes the catalyst easy to absorb moisture and oxidize, which is not conducive to catalytic performance; the above two aspects cause the catalytic performance of the powdered catalyst to be far lower than its theoretical level. Summary of the invention

[0004] [Technical issues]

[0005] The existing catalysts used to synthesize carbon nanotube fibers have inconsistent densities of various components. When they are fed into the high-temperature zone of a high-temperature plasma reaction device through a vibrating feeding device, the various components of the catalyst are separated into layers due to vibration and other reasons, resulting in uneven catalyst components entering the high-temperature zone, which is not conducive to its catalytic performance; the particle size of various components of the existing catalyst is usually 5 to 10 μm, and its specific surface area is large, which makes the catalyst easy to absorb moisture and oxidize, which is not conducive to its catalytic performance; the above two aspects cause the catalytic performance of the powdered catalyst to be far lower than its theoretical level.

[0006] Provided is a granulation method for a catalyst for synthesizing carbon nanotube fibers, wherein the particle strength of the prepared catalyst is not less than 70%, and at the same time, the carbon nanotube fibers synthesized based on the catalyst have a particle strength of not less than 70%. G / I D Not less than 15, ash content not higher than 40, and powder resistance is low.

[0007] [Technical solution]

[0008] In one aspect, a method for pelletizing a catalyst for synthesizing carbon nanotube fibers is provided, comprising the following steps:

[0009] Step 1: Fully mix the raw material powders according to one of the following formulas to obtain a mixed powder; wherein the formula is:

[0010] Iron powder, molybdenum powder and selenium powder, the weight ratio is 1: (0.02-0.04): (0.04-0.08); wherein the iron powder comprises at least one of carbonyl iron powder, atomized iron powder, reduced iron powder, ultrafine iron powder or nano iron powder; or,

[0011] Nano ferric oxide powder and molybdenum sulfide powder, the weight ratio of iron element to sulfur element is 1:(0.034-0.068); or,

[0012] Nano ferric oxide powder and sulfur powder, the weight ratio of iron element to sulfur element is 1:(0.034-0.068);

[0013] Step 2: Mix the binder and the wetting agent to prepare a binder solution with a concentration of 0.5-6 wt %; the decomposition temperature of the binder is 200-300° C.; the wetting agent is a volatile liquid;

[0014] Step 3: Prepare the mixed powder and the binder solution into 20-30 mesh spherical particles by wet granulation; dry to obtain a catalyst for synthesizing carbon nanotube fibers; wherein the weight ratio of the mixed powder to the binder is 100:(0.05-1).

[0015] In some embodiments, the binder includes at least one of ethyl cellulose, dextrin, polyvinyl alcohol, or polyvinylidene fluoride; and the wetting agent includes water or N-methylpyrrolidone.

[0016] In some embodiments, the binder is ethyl cellulose, the wetting agent is N-methylpyrrolidone, and the weight ratio of the mixed powder to the binder is 100:(0.06-0.6); the concentration of the binder solution in step 2 is 0.6-6wt%.

[0017] In some embodiments, the binder is dextrin, the wetting agent is water, and the weight ratio of the mixed powder to the binder is 100:0.1; the concentration of the binder solution in step 2 is 1wt%.

[0018] In some embodiments, the formulation in step 1:

[0019] Iron powder, molybdenum powder and selenium powder, the weight ratio is 1: (0.02-0.04): (0.04-0.08); wherein the iron powder comprises at least one of carbonyl iron powder, atomized iron powder, reduced iron powder, ultrafine iron powder or nano iron powder; or,

[0020] The weight ratio of the nano ferric oxide powder and the molybdenum sulfide powder is 1:(0.034-0.068).

[0021] In some embodiments, the binder is polyvinyl alcohol, the wetting agent is water, and the weight ratio of the mixed powder to the binder is 100:0.1; the concentration of the binder solution in step 2 is 1wt%.

[0022] In some embodiments, the wetting agent is water; step 3 further comprises hydrogen reduction after drying, and the parameters of the hydrogen reduction are: reduction temperature of 300-450°C, gas flow ratio of N2:H2=10:(1-3), reduction time of 30-40min, to obtain the catalyst for synthesizing carbon nanotube fibers.

[0023] In some embodiments, the granulation equipment used in step 3 includes at least one of a ball forming machine, a mixing granulator, an extrusion granulator or a shot blasting machine.

[0024] In some embodiments, the step 3 uses a round pot ball forming machine with a rotation speed of 15 to 20 rpm, sprays the binder solution onto the surface of the mixed powder through a spray gun, and prepares spherical particles of 20 to 30 mesh by rolling.

[0025] In some embodiments, the step 3 uses a mixing granulator, and the mixed powder and the binder solution are respectively added into the barrel of the mixing granulator, and the stirring rate is set to 1000-1500 r / min, the barrel speed is 35 r / min, and high-speed mixing is performed for 1 min; the stirring speed is set to 300-500 r / min, the barrel speed is 30 r / min, and stirring is performed for 3 min to make the mixed powder into spherical particles of 20-30 mesh.

[0026] On the other hand, a catalyst for synthesizing carbon nanotube fibers prepared by the aforementioned method is provided.

[0027] In another aspect, there is provided use of the aforementioned catalyst in synthesizing carbon nanotube fibers.

[0028] [Beneficial Effects]

[0029] The present invention provides a wet granulation method for a catalyst for synthesizing carbon nanotube fibers, wherein the powders of the catalyst components are prepared into spherical particles, so that the different components are adsorbed together by the characteristics of the powders themselves, and bonded together by a binder, a wetting agent, etc. The catalyst granulated by the method of the invention is in the form of spherical particles, which has better fluidity than traditional catalyst powders, and can improve the efficiency of later processing and transmission; it is convenient to use a vibrating feeding device to feed the catalyst later; it effectively prevents the segregation of the catalyst components, and when the high-temperature plasma reaction equipment quickly melts and evaporates the catalyst, the catalyst components will not segregate, ensuring the uniformity of the catalyst and the dispersed distribution of the components; it prevents the catalyst powder from flying and adhering to the reactor wall, which can prevent environmental pollution and catalyst loss.

[0030] The binder selected in the present invention has a low decomposition temperature and can be decomposed at 200-300°C, and can be quickly decomposed during the heat treatment of catalyst particles or during the heating process. The present invention selects a volatile liquid as a wetting agent, and after the wetting agent is dried so that the remaining binder in the catalyst has a very low proportion after the wetting agent volatilizes, the additional carbon content introduced into the catalyst accounts for a very small proportion, and has almost no effect on the catalyst activity, thereby being able to better ensure the catalyst activity.

[0031] After granulation by the method of the present invention, the specific surface area of ​​the catalyst used to synthesize carbon nanotube fibers can be effectively reduced, and under the premise of ensuring the activity of the catalyst, the contact between the catalyst and the air is reduced, the stability and service life of the catalyst are improved, and the plasma method for preparing carbon nanotube fibers can be carried out continuously.

[0032] The method of the present invention realizes the granulation of catalyst powder under the premise of ensuring the activity of the catalyst, and at the same time improves the fluidity of the catalyst. In the method of the present invention, each raw material powder (fine powder) is granulated into macroscopic spherical particles, and the fluidity is greatly improved; after a large number of experimental screenings, the present invention obtains the method of the present invention through the control of the particle size of the granulation, the selection and combination of the binder / wetting agent, the optimization of the dosage, and the optimization design of the granulation equipment and method, which can better ensure the activity of the catalyst and take into account the strength, fluidity and service life of the catalyst particles.

[0033] The particle strength of the catalyst for synthesizing carbon nanotube fibers prepared by the method of the present invention is not less than 70%. At the same time, the carbon nanotube fibers synthesized based on the catalyst have an I G / I D Not less than 15, ash content not higher than 40%, and powder resistance is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a diagram of the finished catalyst product of the present invention.

[0035] Figure 2 Raman image of carbon nanotube fibers prepared using the catalyst of the present invention.

[0036] Figure 3 This is a SEM image of carbon nanotube fibers prepared using the catalyst of the present invention. DETAILED DESCRIPTION

[0037] Example 1

[0038] A method for granulating a catalyst for synthesizing carbon nanotube fibers comprises the following steps:

[0039] Step 1: Use a V-type mixer to premix iron powder, molybdenum powder and selenium powder in a weight ratio of 1:0.04:0.07; then transfer to a high-speed mixer for thorough mixing to obtain a mixed powder for standby use; wherein the iron powder includes: at least one of carbonyl iron powder, atomized iron powder, reduced iron powder, ultrafine iron powder or nano iron powder;

[0040] Step 2: Mix dextrin (as a binder) and pure water (as a wetting agent) in different proportions, cook at 95-100° C. to form a paste-like dextrin solution for later use; wherein the concentrations of the dextrin solution are 1wt%, 1.5wt% and 3wt% respectively;

[0041] Step 3: Use a round pot ball forming machine with a rotation speed of 15 to 20 r / min to spray dextrin solution of 10% by weight of the mixed powder onto the surface of the mixed powder through a spray gun, and prepare spherical particles of 20 to 30 mesh by rolling; dry the spherical particles in a nitrogen atmosphere, and reduce them with hydrogen (reduction temperature is 400°C, gas flow ratio is N2:H2=10:1, and reduction time is 40 min) to obtain catalyst particles for synthesizing carbon nanotube fibers.

[0042] Example 2

[0043] A method for granulating a catalyst for synthesizing carbon nanotube fibers, referring to Example 1, except that in step 1:

[0044] The powder raw material is replaced with nano ferric oxide powder and molybdenum sulfide powder, wherein the weight ratio of Fe element to S element of the nano ferric oxide powder and molybdenum sulfide powder is 1:0.068;

[0045] Alternatively, the powder raw material is replaced with nano ferric oxide powder and sulfur powder, wherein the weight ratio of Fe element to S element in the nano ferric oxide powder and sulfur powder is 1:0.068.

[0046] Example 3

[0047] A method for granulating a catalyst for synthesizing carbon nanotube fibers is described with reference to Example 1, except that in step 2, the binder dextrin is replaced with PVA, and the concentrations of the PVA solution are 1wt%, 1.5wt% and 3wt%.

[0048] Example 4

[0049] A method for granulating a catalyst for synthesizing carbon nanotube fibers, referring to Example 1, differs only in that:

[0050] Step 2: Replace the binder dextrin with the binder ethyl cellulose (EC); replace the pure water with N-methylpyrrolidone (NMP); dissolve EC in NMP to obtain an EC solution for standby use, and the concentration of the EC solution is 0.6wt%;

[0051] Step 3: Using a round pot ball forming machine, spray 10% of the EC solution by weight of the mixed powder onto the surface of the mixed powder through a spray gun, and prepare spherical particles of 20 to 30 mesh by rolling; vacuum dry the spherical particles until solidified to obtain catalyst particles for synthesizing carbon nanotube fibers.

[0052] Example 5

[0053] A method for granulating a catalyst for synthesizing carbon nanotube fibers, referring to Example 4, differs only in that:

[0054] The concentration of EC solution in step 2 is 6 wt %.

[0055] Example 6

[0056] A method for granulating a catalyst for synthesizing carbon nanotube fibers, referring to Example 5, differs only in that:

[0057] Step 3: Add 4 kg of mixed powder and 10% of the EC solution by weight of the powder into the barrel of the mixing granulator, set the stirring rate to 1000-1500 r / min, the barrel speed to 35 r / min, and mix at high speed for 1 min; set the stirring speed to 300-500 r / min, the barrel speed to 30 r / min, and stir for 3 min to make the powder into spherical particles of 20-30 mesh, and vacuum dry the spherical particles until solidified to obtain catalyst particles for synthesizing carbon nanotube fibers.

[0058] Example 7

[0059] A method for granulating a catalyst for synthesizing carbon nanotube fibers, referring to Example 1, differs only in that:

[0060] In step 2, the binder dextrin is replaced with polyvinylidene fluoride (PVDF), and the pure water is replaced with NMP; PVDF is dissolved in NMP to obtain a PVDF solution for standby use, and the concentration of the PVDF solution is 6wt%;

[0061] Step 3: Using a round pot ball forming machine, spray PVDF solution of 10% of the weight of the mixed powder onto the surface of the mixed powder through a spray gun, and prepare spherical particles of 20 to 30 mesh by rolling; vacuum dry the spherical particles until solidified to obtain catalyst particles for synthesizing carbon nanotube fibers.

[0062] Comparative Example 1

[0063] A catalyst powder for synthesizing carbon nanotube fibers, referring to Example 1, except that:

[0064] Steps 2 and 3 are omitted, and the mixed powder is directly used as catalyst powder for synthesizing carbon nanotube fibers.

[0065] Example 8

[0066] The use of the catalyst particles prepared in Examples 1 to 7 or the catalyst powder prepared in Comparative Example 1 in preparing carbon nanotube fibers comprises the following steps:

[0067] The catalyst particles prepared in Examples 1 to 7 or the catalyst powder prepared in Comparative Example 1 are fed into a high-temperature plasma reaction device at a feeding rate of 1 to 2 g / min using a vibrating feeding device, and carbon nanotube fibers are prepared according to the preparation process of patent CN112250061A, except that the composition of the organic carbon source mixed gas is as follows: methane: 4 to 10%, water vapor: 0 to 1%, argon 85 to 90%, hydrogen 1 to 5%, and the total gas flow rate is 100 to 1000 L / min.

[0068] The properties of the carbon nanotube fibers synthesized by the catalysts prepared by the methods of the various examples and comparative examples in Example 8 were tested, and the results are shown in Table 1. Among them:

[0069] I G / I D : refers to the intensity of the G peak in the Raman spectrum (I G ) and D peak intensity (I D ) ratio; measured by Raman spectrometer I G and I D , calculate I G / I D I G / I D The larger the value, the higher the crystallinity of the carbon nanotube fiber product.

[0070] Ash content: refers to the weight percentage of the residue obtained by completely oxidizing and decomposing the carbon element in the product under high temperature and oxygen conditions to the original product; it is measured using the rapid ash method; the lower the ash content, the higher the purity of the nanotube fiber product.

[0071] Powder resistance: refers to the resistance value obtained by pressing the nanotube fiber product powder into a flat sheet less than 4mm and testing it with a four-probe resistance meter; the smaller the powder resistance value is tested with a four-probe resistance meter, the better the conductive performance of the nanotube fiber product.

[0072] Catalyst strength: Randomly select a certain number of finished catalyst particles after granulation, let them fall freely from a height of 70 to 80 cm, and count the proportion of intact particles.

[0073] Table 1

[0074]

[0075] Among them, / indicates that the corresponding test was not performed.

[0076] The study found that no matter what kind of binder is selected, the quality of the carbon nanotube fiber product obtained from the granulated catalyst is better than that of the ungranulated powdered catalyst. This is due to the limitations of the high-temperature plasma reaction equipment, which makes it impossible to uniformly and stably deliver the ungranulated powdered catalyst to the high-temperature area, resulting in poor catalytic performance of the ungranulated powdered catalyst: the I G / I D The ash content is much lower than that of the granulated catalyst of the present invention. The ash content varies according to the reaction conditions. The upper limit of the ash content of the product obtained by most granulated catalysts is lower than that of the ungranulated catalysts. The lowest value of the powder resistance of the product obtained by the ungranulated catalysts is still higher than that of most granulated catalysts. As shown in Example 4, the product I obtained by using 0.6wt% EC G / I D The maximum value can reach 120, which is 8 to 24 times higher than that of ungranulated catalyst powder. The ash content is less than 10%, and the powder resistance is less than 15mΩ·cm -1 , the catalyst particle strength is as high as 89%. As shown in Example 6, using 6wt% EC, the product I G / I D The maximum value can reach 70, which is 5 to 14 times higher than that of ungranulated catalyst powder. The ash content is less than 10%, and the powder resistance is less than 15 mΩ·cm -1 , the catalyst particle strength is as high as 95%.

[0077] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for granulating a catalyst for synthesizing carbon nanotube fibers, characterized in that: The steps include: Step 1: Fully mix the raw material powders according to one of the following formulas to obtain a mixed powder; wherein the formula is: Iron powder, molybdenum powder and selenium powder, the weight ratio is 1: (0.02-0.04): (0.04-0.08); wherein the iron powder comprises at least one of carbonyl iron powder, atomized iron powder, reduced iron powder, ultrafine iron powder or nano iron powder; or, Nano ferric oxide powder and molybdenum sulfide powder, the weight ratio of iron element to sulfur element is 1:(0.034-0.068); or, Nano ferric oxide powder and sulfur powder, the weight ratio of iron element to sulfur element is 1:(0.034-0.068); Step 2: Mix the binder and the wetting agent to prepare a binder solution with a concentration of 0.5-6 wt %; the decomposition temperature of the binder is 200-300° C.; the wetting agent is a volatile liquid; Step 3: Prepare the mixed powder and the binder solution into 20-30 mesh spherical particles by wet granulation; dry to obtain a catalyst for synthesizing carbon nanotube fibers; wherein the weight ratio of the mixed powder to the binder is 100:(0.05-1).

2. The method according to claim 1, characterized in that The binder includes at least one of ethyl cellulose, dextrin, polyvinyl alcohol or polyvinylidene fluoride; and the wetting agent includes water or N-methylpyrrolidone.

3. The method according to claim 1, characterized in that: The binder is ethyl cellulose, the wetting agent is N-methylpyrrolidone, the weight ratio of the mixed powder to the binder is 100:(0.06-0.6); the concentration of the binder solution in step 2 is 0.6-6wt%.

4. The method according to claim 1, characterized in that The binder is dextrin, the wetting agent is water, and the weight ratio of the mixed powder to the binder is 100:0.1; the concentration of the binder solution in step 2 is 1wt%.

5. The method according to claim 4, characterized in that The recipe described in step 1: Iron powder, molybdenum powder and selenium powder, the weight ratio is 1: (0.02-0.04): (0.04-0.08); wherein the iron powder comprises at least one of carbonyl iron powder, atomized iron powder, reduced iron powder, ultrafine iron powder or nano iron powder; or, The weight ratio of the nano ferric oxide powder and the molybdenum sulfide powder is 1:(0.034-0.068).

6. The method according to claim 1, characterized in that The binder is polyvinyl alcohol, the wetting agent is water, and the weight ratio of the mixed powder to the binder is 100:0.1; the concentration of the binder solution in step 2 is 1wt%.

7. The method according to claim 1, characterized in that The wetting agent is water; step 3 also includes hydrogen reduction after drying, the parameters of the hydrogen reduction are: reduction temperature is 300-450°C, gas flow ratio is N2:H2=10:(1-3), reduction time is 30-40min, and the catalyst for synthesizing carbon nanotube fibers is obtained.

8. The method according to claim 1, characterized in that The granulation equipment used in step 3 includes at least one of a ball forming machine, a mixing granulator, an extrusion granulator or a shot blasting machine.

9. A catalyst for synthesizing nanotube fibers obtained by the method according to any one of claims 1 to 8.

10. Use of the catalyst according to claim 9 in synthesizing carbon nanotube fibers.

Citation Information

Patent Citations

  • Preparation method of carbon nanotube catalyst

    CN116603531A

  • Device for reversing laver farming net

    KR1020220128096A

  • Preparation method of carbon nanotubes

    KR102230243B1

  • Transition metal catalyst supported by a substrate, production method thereof and use of same for the production of carbon nanotubes

    WO2013083928A1