Silicon nitride loaded metal nanoparticle composite material as well as preparation method and application thereof

By depositing metal nanoparticles such as Ni, Co and Fe on the silicon nitride support, and using the strong interaction of Si3N4 support, the problem of poor stability of metal-based nanocatalysts at high temperatures is solved, and an efficient ammonia decomposition and hydrogen production reaction is achieved. The catalyst exhibits high conversion and high catalytic activity.

CN118904378AInactive Publication Date: 2024-11-08INST OF COAL CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410955925.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing metal-based nanocatalysts are prone to Osterwald maturation under high temperature conditions, resulting in poor catalytic stability and difficult to achieve high loading and high dispersion, which limits their application in ammonia decomposition and hydrogen production reaction.

Method used

Silicon nitride is used as a carrier to prepare metal nanoparticles such as Ni, Co and Fe through precipitation and deposition. The strong interaction between Si3N4 carrier and transition metal is used to achieve high dispersion and small particle size of metal nanoparticles to avoid agglomeration. , and optimize the structure of the catalyst through the calcination and reduction steps.

Benefits of technology

The high conversion rate and high catalytic activity in the ammonia decomposition reaction at high temperature were achieved, the NH3 conversion rate of the catalyst reached 98.6%, and the hydrogen production rate reached 66.0 mmol/gcat/min, which significantly improved the efficiency and catalytic reaction of ammonia decomposition and hydrogen production. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904378A_ABST
    Figure CN118904378A_ABST
Patent Text Reader

Abstract

The invention provides a silicon nitride loaded metal nanoparticle composite material as well as a preparation method and application thereof, and belongs to the technical field of metal nano-catalysts. The silicon nitride loaded metal nanoparticle composite material comprises a silicon nitride carrier and metal nanoparticles dispersed on the silicon nitride carrier, the metal nanoparticles comprise one or more of Ni, Co and Fe. In the silicon nitride loaded metal nanoparticle composite material provided by the invention, strong metal carrier interaction exists between the transition metals Ni, Co and Fe and the Si3N4 carrier, and the Si3N4 carrier can anchor the transition metals, so that the active metals are small in particle size and high in dispersity, agglomeration is prevented due to the strong metal carrier interaction, and the metal nanoparticles can be dispersed in the active metals. And the conversion rate of catalyzing ammonia decomposition is high when the catalyst is used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal nanocatalysts, and specifically relates to a silicon nitride-loaded metal nanoparticle composite material and a preparation method and application thereof. Background Art

[0002] H 2 As a clean energy source, it has attracted widespread attention due to its high gravimetric energy content and zero carbon emissions. However, due to its low energy density and low boiling point, it is very difficult to transport and directly store hydrogen. These problems can be overcome by using hydrogen carriers, making it easier to transport to consumption areas and reform or decompose on site to produce hydrogen. Ammonia has high hydrogen storage density (17.7wt%), easy liquefaction (0.8MPa), mature transportation technology, low hydrogen production cost, and no CO2 when decomposed. x It has the advantages of production and is considered to be one of the ideal hydrogen storage carriers.

[0003] At present, Ru-based catalysts are considered to be the best catalysts for hydrogen production by ammonia decomposition, but the high cost of Ru limits its large-scale industrial application. Ni, Co and Fe-based catalysts are non-precious metal catalysts with higher activity in ammonia decomposition and are a good choice commercially. However, due to thermodynamic and kinetic limitations, ammonia decomposition requires higher temperatures (e.g., 500-700°C) to achieve high conversion rates under high space velocity conditions, and active components are prone to agglomeration under high temperature conditions.

[0004] Metal-based nanocatalysts have received extensive attention in recent decades, which is attributed to their high catalytic intrinsic activity brought about by their large metal dispersion and nano-effect. However, due to the high coordination unsaturation of small nanoparticles, they are prone to Ostwald ripening (i.e., particle size growth) under harsh high temperatures, resulting in poor catalytic stability. People have tried many methods to achieve effective control of particle size, such as: using atomic deposition (ALD) to prepare single-atom catalysts, but its cost is high, catalyst yield is low, and the preparation is complex and the active component loading is low; in addition, although the ALD method has advantages in turnover frequency (TOF) value and metal dispersion, the performance of the catalyst per unit mass is poor, and the practical application significance of base metal catalysts is limited; for example: using metal oxides as carriers to load active components to prepare catalysts, relying on CeO 2 The strong interaction between CeO and metal supports, although the metal particle size is small, 2 The thermal stability is poor, and the covering effect with the metal results in low dispersion.

[0005] Therefore, there is an urgent need to provide a metal-based nanocatalyst with high loading, small particle size, and high dispersion, which is of great significance for the practical application of reactions such as high-temperature ammonia decomposition. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a silicon nitride-supported metal nanoparticle composite material and a preparation method and application thereof. The silicon nitride-supported metal nanoparticle composite material provided by the present invention can enable the metal nanoparticles to achieve the advantages of high dispersion and small particle size at a high loading amount, and effectively prevent the metal nanoparticles from agglomerating under high-temperature conditions of ammonia decomposition, thereby reducing the catalytic performance.

[0007] In order to achieve the above object, the present invention provides the following scheme:

[0008] The invention provides a silicon nitride-loaded metal nanoparticle composite material, comprising a silicon nitride carrier and metal nanoparticles dispersed on the silicon nitride carrier; the metal nanoparticles comprise one or more of Ni, Co and Fe.

[0009] Preferably, in the silicon nitride-supported metal nanoparticle composite material, the content of the metal nanoparticles is 15-25 wt %.

[0010] Preferably, the average particle size of the metal nanoparticles is 4.0 to 5.2 nm, and the dispersion degree of the metal nanoparticles is 9.1 to 13.2%.

[0011] The present invention provides a method for preparing the silicon nitride-supported metal nanoparticle composite material described in the above scheme, comprising the following steps:

[0012] Mixing a water-soluble metal salt, water, silicon nitride and a precipitant to form a metal hydroxide precipitate on the surface of the silicon nitride, and performing solid-liquid separation to obtain silicon nitride-loaded metal hydroxide; the water-soluble metal salt includes one or more of a water-soluble nickel salt, a water-soluble cobalt salt and a water-soluble iron salt;

[0013] In an inert atmosphere, calcining the silicon nitride-supported metal hydroxide to obtain a silicon nitride-supported metal oxide;

[0014] The silicon nitride-supported metal oxide is reduced in a reducing atmosphere to obtain the silicon nitride-supported metal nanoparticle composite material.

[0015] Preferably, the water-soluble nickel salt comprises Ni(NO 3 ) 2 6H 2 O、NiCl 2 6H 2 O and NiSO 4 7H 2 O; the water-soluble cobalt salt includes Co(NO 3 ) 2 6H 2 O、CoCl2 6H 2 O and CoSO 4 ·xH 2 O; the water-soluble iron salt includes Fe(NO 3 ) 3 9H 2 O, FeCl 3 6H 2 O and Fe 2 (SO 4 ) 3 ·xH 2 One or more of O.

[0016] Preferably, the precipitant comprises Na 2 CO 3 solution, ammonia or NaOH solution.

[0017] Preferably, the mixing temperature is 70°C.

[0018] Preferably, the inert atmosphere includes nitrogen atmosphere, argon atmosphere or helium atmosphere; the calcination temperature is 500-700° C., and the calcination time is 1-6 hours.

[0019] Preferably, the reducing atmosphere comprises a hydrogen atmosphere; the reducing temperature is 500 to 700° C., and the reducing time is 1 to 6 hours.

[0020] The present invention provides the use of the silicon nitride-supported metal nanoparticle composite material described in the above scheme or the silicon nitride-supported metal nanoparticle composite material prepared by the preparation method described in the above scheme as a catalyst in hydrogen production by decomposing ammonia.

[0021] The present invention provides a silicon nitride supported metal nanoparticle composite material, comprising a silicon nitride carrier and metal nanoparticles dispersed on the silicon nitride carrier; the metal nanoparticles include one or more of Ni, Co and Fe. In the silicon nitride supported metal nanoparticle composite material provided by the present invention, due to the transition metals Ni, Co and Fe and Si 3 N 4 There is a strong metal-support interaction between the supports, and Si 3 N 4 The carrier can anchor the transition metal, thus resulting in a small active metal particle size and high dispersion. The strong metal-carrier interaction prevents agglomeration, thereby enabling a high conversion rate for catalytic ammonia decomposition when used as a catalyst.

[0022] The Si provided by the present invention 3 N 4Compared with oxide materials commonly used as catalyst carriers, silicon nitride has better thermal stability, chemical stability and high thermal conductivity. In endothermic reactions at high temperatures, it can promote heat transfer, thereby limiting the formation of local reaction cold spots and preventing the activity of active sites from decreasing. 3 N 4 The carrier can enable the ammonia decomposition hydrogen production reaction at high temperature to have a high conversion rate.

[0023] The present invention adopts precipitation deposition method (DP) to prepare silicon nitride loaded metal nanoparticle composite material, wherein the average particle size of the metal nanoparticles is 4.0-5.2nm, which is better than other oxide carriers and solves the technical difficulty of achieving high dispersion and small particle size under high loading amount.

[0024] For the high-temperature ammonia decomposition reaction to produce hydrogen, the activity of silicon nitride-supported metal nanoparticle composites as catalysts is higher than that of currently commonly used metal oxide supports (such as Al 2 O 3 、SiO 2 ,La 2 O 3 、CeO 2 and TiO 2 ) catalyst; at a space velocity of 60000mL / g cat / h, 650℃, the NH 3 The conversion rate reached 98.6% and the hydrogen production rate reached 66.0mmol / g cat / min; and with the increase of reaction time, within 60h, NH 3 The conversion rate remains basically unchanged.

[0025] The ammonia decomposition catalyst of the present invention is an important technological breakthrough. Its high catalytic activity and high space velocity improve the efficiency of ammonia decomposition. The space velocity is 60000mL / g cat / h, 98.6% conversion at 650 °C demonstrates its high efficiency at high space velocity.

[0026] The present invention adopts the precipitation deposition method through Si 3 N 4 The carrier is used to prepare a highly efficient high space velocity ammonia decomposition catalyst. The catalyst synthesis process is simple and easy to repeat. The prepared catalyst particles are easy to control and not easy to agglomerate, thereby improving the ammonia decomposition performance of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0028] Figure 1 The Ni / Si 3 N 4 XRD pattern of

[0029] Figure 2 The Ni / Si 3 N 4 TEM images of

[0030] Figure 3 The Ni / Si 3 N 4 and NiO H 2 -TPR graph;

[0031] Figure 4 The catalytic effect comparison diagram of the composite materials obtained in Example 1 of the present invention and Comparative Examples 1 to 5 is shown. DETAILED DESCRIPTION

[0032] The invention provides a silicon nitride-loaded metal nanoparticle composite material, comprising a silicon nitride carrier and metal nanoparticles dispersed on the silicon nitride carrier; the metal nanoparticles comprise one or more of Ni, Co and Fe.

[0033] In the present invention, in the silicon nitride-supported metal nanoparticle composite material, the content of the metal nanoparticles is preferably 15 to 25 wt %, and more preferably 18 to 22 wt %.

[0034] In the present invention, the average particle size of the metal nanoparticles is preferably 4.0 to 5.2 nm; the dispersion of the metal nanoparticles is preferably 9.1 to 13.2%. In the present invention, the dispersion refers to the ratio of the number of active metal atoms on the surface of the silicon nitride-supported metal nanoparticle composite material to the total number of metal atoms on the silicon nitride-supported metal nanoparticle composite material.

[0035] In the silicon nitride loaded metal nanoparticle composite material provided by the present invention, due to the transition metals Ni, Co and Fe and Si 3 N 4 There is a strong metal-support interaction between the supports, and Si 3 N 4The carrier can anchor the transition metal, thus resulting in a small active metal particle size and high dispersion. The strong metal-carrier interaction prevents agglomeration, thereby enabling a high conversion rate for catalytic ammonia decomposition when used as a catalyst.

[0036] The present invention provides a method for preparing the silicon nitride-supported metal nanoparticle composite material described in the above scheme, comprising the following steps:

[0037] Mixing a water-soluble metal salt, water, silicon nitride and a precipitant to form a metal hydroxide precipitate on the surface of the silicon nitride, and performing solid-liquid separation to obtain silicon nitride-loaded metal hydroxide; the water-soluble metal salt includes one or more of a water-soluble nickel salt, a water-soluble cobalt salt and a water-soluble iron salt;

[0038] In an inert atmosphere, calcining the silicon nitride-supported metal hydroxide to obtain a silicon nitride-supported metal oxide;

[0039] The silicon nitride-supported metal oxide is reduced in a reducing atmosphere to obtain the silicon nitride-supported metal nanoparticle composite material.

[0040] Unless otherwise specified, the materials and equipment used in the present invention are commercially available.

[0041] The invention mixes water-soluble metal salt, water, silicon nitride and a precipitant, forms metal hydroxide precipitation on the surface of silicon nitride, separates the solid and the liquid, and obtains silicon nitride-loaded metal hydroxide.

[0042] In the present invention, the water-soluble metal salt includes one or more of a water-soluble nickel salt, a water-soluble cobalt salt and a water-soluble iron salt; the water-soluble nickel salt preferably includes Ni(NO 3 ) 2 6H 2 O、NiCl 2 6H 2 O and NiSO 4 7H 2 O; the water-soluble cobalt salt preferably includes Co(NO 3 ) 2 6H 2 O、CoCl 2 6H 2 O and CoSO 4 ·xH 2 O; the water-soluble iron salt preferably includes Fe(NO 3 ) 3 9H 2 O, FeCl 3 6H 2 O and Fe 2 (SO 4 ) 3·xH 2 One or more of O.

[0043] In the present invention, the precipitant preferably comprises Na 2 CO 3 In the present invention, the Na 2 CO 3 The concentration of the solution is preferably 0.1 mol / L; the ammonia water (NH 3 ·H 2 The mass concentration of O) is preferably 3%; the concentration of the NaOH solution is preferably 0.01 mol / L.

[0044] In the present invention, the mass ratio of the water-soluble metal salt to the volume ratio of water is preferably (2-6) g: (120-180) mL, and more preferably (2.5-5.5) g: (140-160) mL.

[0045] In the present invention, the mass ratio of the water-soluble metal salt to silicon nitride is preferably (1-3):1, and more preferably (1.5-2.5):1.

[0046] The Si provided by the present invention 3 N 4 Compared with oxide materials commonly used as catalyst carriers, silicon nitride has better thermal stability, chemical stability and high thermal conductivity. In endothermic reactions at high temperatures, it can promote heat transfer, thereby limiting the formation of local reaction cold spots and preventing the activity of active sites from decreasing. 3 N 4 The carrier can enable the ammonia decomposition hydrogen production reaction at high temperature to have a high conversion rate.

[0047] In the present invention, the specific surface area of ​​the silicon nitride is preferably 58.7 cm 3 / g, in the embodiments of the present invention, the specific source is Qinhuangdao Yinuo Materials Development Co., Ltd.

[0048] In the present invention, mixing the water-soluble metal salt, water, silicon nitride and the precipitant preferably comprises: dissolving the water-soluble metal salt in water, then adding silicon nitride under stirring, and then dropping the precipitant.

[0049] In the present invention, the mixing temperature is preferably 70°C.

[0050] In the present invention, before adding silicon nitride, the process preferably further comprises vacuum drying the silicon nitride at 180° C. overnight; and the amount of the precipitant preferably satisfies that the pH value of the resulting suspension is 9.

[0051] In the process of dripping the precipitant, nickel ions react with hydroxide ions generated by hydrolysis of carbonate ions to generate green nickel hydroxide precipitates.

[0052] After completing the dropwise addition, the present invention preferably further comprises aging the obtained reaction system.

[0053] In the present invention, the aging time is preferably 2 hours. The present invention can make the metal hydroxide precipitate better attached to the silicon nitride carrier through aging.

[0054] In the present invention, the separation preferably includes centrifugal separation.

[0055] After completing the solid-liquid separation, the present invention preferably further comprises washing and drying the obtained precipitated product in sequence.

[0056] In the present invention, the washing is preferably performed three times with deionized water; the drying temperature is preferably 120° C., and the drying time is preferably 12 hours.

[0057] After obtaining the silicon nitride-supported metal hydroxide, the present invention bakes the silicon nitride-supported metal hydroxide in an inert atmosphere to obtain the silicon nitride-supported metal oxide.

[0058] In the present invention, the inert atmosphere preferably includes nitrogen atmosphere, argon atmosphere or helium atmosphere. In the present invention, the calcination temperature is preferably 500-700°C, more preferably 550-650°C, more preferably 580-630°C; the calcination time is preferably 1-6h, more preferably 1.5-4.5h, more preferably 2-4h.

[0059] In the process of calcination, the metal hydroxide is dehydrated to become metal oxide. In the calcination product, the content of the carrier silicon nitride is 65-75wt% based on the mass of the metal oxide supported by silicon nitride, and the content of the active component in metal state is 17-21wt%.

[0060] The silicon nitride-loaded metal oxide is obtained. In the present invention, the silicon nitride-loaded metal oxide is reduced in a reducing atmosphere to obtain the silicon nitride-loaded metal nanoparticle composite material.

[0061] In the present invention, the reducing atmosphere preferably includes a hydrogen atmosphere. In the present invention, the reducing temperature is preferably 500-700°C, more preferably 550-650°C, more preferably 580-630°C; the reducing time is preferably 1-6h, more preferably 1.5-4.5h, more preferably 2-4h.

[0062] In the reduction process of the present invention, the silicon nitride-loaded metal oxide is reduced to a metal element.

[0063] The ammonia decomposition catalyst of the present invention is an important technological breakthrough. Its high catalytic activity and high space velocity improve the efficiency of ammonia decomposition. The space velocity is 60000mL / g cat / h, 98.6% conversion at 650 °C demonstrates its high efficiency at high space velocity.

[0064] The present invention adopts the precipitation deposition method through Si 3 N 4 The carrier is used to prepare a highly efficient high space velocity ammonia decomposition catalyst. The catalyst synthesis process is simple and easy to repeat. The prepared catalyst particles are easy to control and not easy to agglomerate, thereby improving the ammonia decomposition performance of the catalyst.

[0065] The present invention provides the use of the silicon nitride-supported metal nanoparticle composite material described in the above scheme or the silicon nitride-supported metal nanoparticle composite material prepared by the preparation method described in the above scheme as a catalyst in hydrogen production by decomposing ammonia.

[0066] In the present invention, the temperature for producing hydrogen by decomposing ammonia is preferably 400-700°C, and more preferably 450-650°C.

[0067] The present invention has no special requirements for the application steps, and methods well known in the art can be used. In the embodiment of the present invention, 100 mg of catalyst (40-60 mesh) and 200 mg of quartz sand (40-60 mesh) are mixed and loaded into a quartz tube (6 mm ID), and then ammonia is decomposed to produce hydrogen.

[0068] Before the application, the present invention also preferably comprises the step of: subjecting the obtained silicon nitride-supported metal nanoparticle composite material to H 2 Reduction in atmosphere.

[0069] In the present invention, the flow rate of the hydrogen is preferably 100 mL / min; the reduction temperature is preferably 600°C, and the time is preferably 2 h; the reduction is preferably heated from room temperature to the reduction temperature, and the heating rate is preferably 5°C / min.

[0070] In the present invention, all catalyst evaluations (i.e., applications) were conducted in the temperature range of 400-700°C with a step length of 50°C. The ammonia gas hourly space velocity (GHSV) was 60000 mL / g cat / h. The obtained gas H was analyzed by gas chromatograph (Aglient7890B). 2 Conduct analysis.

[0071] Ammonia (X NH3 ) conversion rate and hydrogen production rate (rH2 ) is calculated according to Formula 1 and Formula 2.

[0072]

[0073] Among them, [V H2 ] is the product H 2 Volume percentage; F NH3 is the inlet ammonia flow rate (mL / min), M cat is the mass of the catalyst (g).

[0074] The XRD testing equipment used for the catalyst in the present invention is Bruker D 8Advance XRD, the target material is Co target, the current is 25 mA, and the voltage is 40 kV.

[0075]

[0076] Where k (k = 0.89) is the Scherrer constant, β is the half maximum width (FWHM) of the active metal diffraction peak, and θ represents the diffraction angle.

[0077] To further illustrate the present invention, a silicon nitride-loaded metal nanoparticle composite material and its preparation method and application provided by the present invention are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.

[0078] In the embodiments and comparative examples of the present invention, Si 3 N 4 SiO was purchased from Qinhuangdao Yinuo High-tech Materials Development Co., Ltd. 2 ,La 2 O 3 and CeO 2 Purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. 2 O 3 Ni(NO 3 ) 2 6H 2 O、Co(NO 3 ) 2 6H 2 O, Fe(NO 3 ) 3 9H 2 O and Na 2 CO 3 Purchased from China National Pharmaceutical Group Co., Ltd. Deionized water used in all experiments was homemade in the laboratory.

[0079] Example 1

[0080] Preparation of silicon nitride-supported metal nanoparticle composites: Weigh 2.66 g Ni(NO 3 ) 2 6H 2 O was dissolved in 150 mL of deionized water, and then 2.0 g of silicon nitride carrier dried overnight at 180 °C was added to the solution under stirring. 2 CO 3 The precipitant was added dropwise to the suspension until the pH value of the suspension was 9, and the addition was stopped. The resulting suspension was stirred and aged at 70°C for 2 h. The resulting precipitate was centrifuged, washed three times with deionized water, dried at 120°C in vacuum for 12 h, and calcined at 600°C in Ar for 2 h to obtain the target product Ni / Si 3 N 4 , where Ni is in Ni / Si 3 N 4 The theoretical loading amount in the sample is 20 wt % and the actual loading amounts are summarized in Table 1.

[0081] Ni / Si 3 N 4 Evaluation of catalysts for hydrogen production from ammonia decomposition: In the evaluation experiment, 100 mg of silicon nitride-supported metal nanoparticle composite material as a catalyst (40-60 mesh) was mixed with 200 mg of quartz sand (40-60 mesh) and loaded into a quartz tube (6 mm ID). Before the evaluation, the catalyst was heated in H 2 (100mL / min) was heated to 600℃, the heating rate was 5℃ / min, and the reduction was carried out at 600℃ for 2h. The catalyst evaluation was carried out in the temperature range of 400-700℃, with a step length of 50℃. cat / h and 650℃, the ammonia conversion rate is 98.6%. cat / h and 650℃, the ammonia conversion rate is 99.8%.

[0082] Example 2

[0083] Preparation of silicon nitride-supported metal nanoparticle composites: 2.65 g Co(NO 3 ) 2 6H 2 O was dissolved in 150 mL of deionized water, and then 2.0 g of silicon nitride carrier dried overnight in vacuum at 180 ° C was added to the solution under stirring; the prepared 0.1 mol / L Na 2 CO 3The precipitant was added dropwise to the suspension until the pH value of the suspension was 9, and the addition was stopped. The resulting suspension was stirred and aged at 70°C for 2 h. The resulting precipitate was centrifuged, washed three times with deionized water, dried at 120°C in vacuum for 12 h, calcined at 600°C in Ar for 2 h, and then heated at 600°C in H 2 The target product Co / Si was obtained by reduction for 2 h. 3 N 4 , among which Co in Co / Si 3 N 4 The theoretical loading amount in the sample is 20 wt % and the actual loading amounts are summarized in Table 1.

[0084] Co / Si 3 N 4 Evaluation of catalysts for hydrogen production from ammonia decomposition: In the evaluation experiment, 100 mg of silicon nitride-supported metal nanoparticle composite material as a catalyst (40-60 mesh) was mixed with 200 mg of quartz sand (40-60 mesh) and loaded into a quartz tube (6 mm ID). Before the evaluation, the catalyst was heated in H 2 (100mL / min) was heated to 600℃, the heating rate was 5℃ / min, and the reduction was carried out at 600℃ for 2h. cat / h and 650℃, the ammonia conversion rate is 92.8%. cat / h and 650℃, the ammonia conversion rate is 99.5%.

[0085] Example 3

[0086] Preparation of silicon nitride-supported metal nanoparticle composites: Weigh 4.05 g Fe(NO 3 ) 3 9H 2 O was dissolved in 150 mL of deionized water, and then 2.0 g of silicon nitride carrier dried overnight in vacuum at 180 °C was added to the solution under stirring. 3 ·H 2 O precipitant was added dropwise to the above suspension until the pH value of the suspension was 10, and the addition was stopped. The resulting suspension was stirred and aged at 70°C for 2h. The resulting precipitate was centrifuged, washed three times with deionized water, vacuum dried at 120°C for 12h, calcined at 600°C in Ar for 2h, and then heated at 600°C in H 2 The target product Fe / Si was obtained by reduction for 2 h. 3 N 4 , where Fe is in Fe / Si 3 N 4 The theoretical loading amount in the sample is 20 wt % and the actual loading amounts are summarized in Table 1.

[0087] Fe / Si 3N 4 Evaluation of catalysts for hydrogen production from ammonia decomposition: In the evaluation experiment, 100 mg of silicon nitride-supported metal nanoparticle composite material as a catalyst (40-60 mesh) was mixed with 200 mg of quartz sand (40-60 mesh) and loaded into a quartz tube (6 mm ID). Before the evaluation, the catalyst was heated in H 2 (100mL / min) was heated to 600℃, the heating rate was 5℃ / min, and the reduction was carried out at 600℃ for 2h. cat / h and 650℃, the ammonia conversion rate is 88.4%. cat / h and 650℃, the ammonia conversion rate is 99.2%.

[0088] Comparative Example 1

[0089] Other conditions are the same as those in Example 1. The carrier of the silicon nitride-supported metal nanoparticle composite material is Al 2 O 3 . At 60000mL / g cat / h and 650℃, the ammonia conversion rate is 81.0%.

[0090] Comparative Example 2

[0091] The other conditions were the same as those in Example 1. The carrier of the silicon nitride-supported metal nanoparticle composite material was SiO 2 . At 60000mL / g cat / h and 650℃, the ammonia conversion rate is 73.9%.

[0092] Comparative Example 3

[0093] Other conditions are the same as those in Example 1. The carrier of the silicon nitride-supported metal nanoparticle composite material is La 2 O 3 . At 60000mL / g cat / h and 650℃, the ammonia conversion rate is 54.3%.

[0094] Comparative Example 4

[0095] Other conditions are the same as those in Example 1. The carrier of the silicon nitride-supported metal nanoparticle composite material is CeO 2 . At 60000mL / g cat / h and 650℃, the ammonia conversion rate is 43.0%.

[0096] Comparative Example 5

[0097] Other conditions were the same as those in Example 1, except that the carrier of the silicon nitride-supported metal nanoparticle composite material was TiO 2 . At 60000mL / g cat / h and 650℃, the ammonia conversion rate is 38.1%.

[0098] Performance testing and structural characterization

[0099] Table 1 shows the structural information of the silicon nitride-supported metal nanoparticle composite materials of Examples 1 to 3 and Comparative Examples 1 to 5 and the cat / h space velocity and ammonia conversion information at 650℃.

[0100] Table 1 Summary of the material structures and ammonia conversion rates obtained in Examples 1 to 3 and Comparative Examples 1 to 5

[0101]

[0102]

[0103] As can be seen from Table 1, the silicon nitride-supported metal nanoparticle composite material prepared in the present invention can enable the metal nanoparticles to achieve the advantages of high dispersion and small particle size at a high loading amount, and has a high ammonia conversion rate.

[0104] The Ni nanocatalyst prepared in Example 1 was characterized and analyzed, wherein the characterization analysis included: X-ray diffractometer (XRD), transmission electron microscope (TEM), programmed temperature reduction (HT 2 -TPR) and physical adsorption instrument (BET).

[0105] Figure 1 is the Ni / Si in Example 1 of the present invention 3 N 4 X-ray diffraction pattern of catalyst, Ni / Si 3 N 4 The catalyst XRD spectrum has three diffraction peaks at 2θ of 52.2°, 61.0°, and 91.8°, corresponding to Ni(111), Ni(200), and Ni(220) planes, respectively. According to the Scherrer formula, the half-peak width of Ni is wider, indicating that the Ni particle size is smaller.

[0106] Transmission electron microscopy (TEM) was measured using a Talos 200A (FEI, USA). Figure 2 is the Ni / Si in Example 1 of the present invention 3 N 4 TEM image of the catalyst. As shown in the figure, Ni particles are evenly dispersed on Si 3 N 4 On the carrier, the average particle size of Ni is 4.0nm, and the surface Ni / Si 3 N 4 The catalyst has the advantages of small particle size and high dispersibility.

[0107] H2 -TPR was performed in AutoChem IIASAP 2950. About 50 mg of sample was placed in a U-shaped quartz tube reactor. The sample was pretreated with argon (50 mL / min) at 300 °C for 1 hour, then cooled to 40 °C and 10% H 2 / He (50mL / min). The heating rate from 40℃ to 800℃ was kept constant (10℃ / min). A thermal conductivity detector (TCD) was used to monitor the change of outlet gas concentration. Isopropyl alcohol gel was used to remove water. Figure 3 is the Ni / Si in Example 1 of the present invention 3 N 4 Catalyst and NiO H 2 -TPR diagram. Ni / Si 3 N 4 The temperature for hydrogen reduction of NiO to Ni in the catalyst is 636°C, while the temperature for hydrogen reduction of NiO to Ni in NiO is 360°C and 20Ni / Si 3 N 4 The catalyst reduction temperature is high, possibly due to the Ni and Si 3 N 4 There is a strong metal-support interaction between the supports, resulting in a small Ni particle size and high dispersion.

[0108] Figure 4 The catalytic effect comparison diagram of the catalysts of Example 1 of the present invention and Comparative Examples 1 to 5 is shown in FIG. cat / h airspeed compared with 20Ni / Si 3 N 4 、20Ni / Al 2 O 3 、20Ni / SiO 2 、20Ni / La 2 O 3 、20Ni / CeO 2 and 20Ni / TiO 2 The catalyst (where 20 represents the theoretical loading amount of Ni on the catalyst silicon nitride supported metal nanoparticle composite material is 20wt%) 3 The catalytic performance of decomposition of NH 3 The conversion rate of NH 3 The exothermic nature of the decomposition reaction is consistent. In the range of 400-700℃, 20Ni / Si 3 N 4 The catalyst activity is higher than other supported catalysts. The performance of nickel-based catalysts on different supports is 20Ni / Si 3 N 4 >20Ni / Al 2 O3 >20Ni / SiO 2 >20Ni / La 2 O 3 >20Ni / CeO 2 >20Ni / TiO 2 . At 60000mL / g cat / h air velocity, at 650℃, 20Ni / Si 3 N 4 NH on the catalyst 3 The conversion rate reached 98.6% and the hydrogen production rate reached 66.0mmol / g cat / min. Therefore, 20Ni / Si 3 N 4 The catalyst is a very good catalyst for the decomposition of ammonia to produce hydrogen.

[0109] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A silicon nitride-loaded metal nanoparticle composite material, It is characterized in that It comprises a silicon nitride carrier and metal nanoparticles dispersed on the silicon nitride carrier; the metal nanoparticles comprise one or more of Ni, Co and Fe.

2. The silicon nitride-supported metal nanoparticle composite material according to claim 1, It is characterized in that In the silicon nitride-supported metal nanoparticle composite material, the content of the metal nanoparticles is 15-25 wt %.

3. The silicon nitride-supported metal nanoparticle composite material according to claim 1, It is characterized in that The average particle size of the metal nanoparticles is 4.0-5.2 nm, and the dispersion degree of the metal nanoparticles is 9.1-13.2%.

4. A method for preparing the silicon nitride-supported metal nanoparticle composite material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Mixing a water-soluble metal salt, water, silicon nitride and a precipitant to form a metal hydroxide precipitate on the surface of the silicon nitride, and performing solid-liquid separation to obtain silicon nitride-loaded metal hydroxide; the water-soluble metal salt includes one or more of a water-soluble nickel salt, a water-soluble cobalt salt and a water-soluble iron salt; In an inert atmosphere, calcining the silicon nitride-supported metal hydroxide to obtain a silicon nitride-supported metal oxide; The silicon nitride-supported metal oxide is reduced in a reducing atmosphere to obtain the silicon nitride-supported metal nanoparticle composite material.

5. The preparation method according to claim 4, It is characterized in that The water-soluble nickel salt includes Ni(NO 3 ) 2 6H 2 O、NiCl 2 6H 2 O and NiSO 4 7H 2 O; the water-soluble cobalt salt includes Co(NO 3 ) 2 6H 2 O、CoCl 2 6H 2 O and CoSO 4 ·xH 2 O; the water-soluble iron salt includes Fe(NO 3 ) 3 9H 2 O, FeCl 3 6H 2 O and Fe 2 (SO 4 ) 3 ·xH 2 One or more of O.

6. The preparation method according to claim 4 or 5, It is characterized in that The precipitant includes Na 2 CO 3 solution, ammonia or NaOH solution.

7. The preparation method according to claim 4 or 5, It is characterized in that The mixing temperature was 70°C.

8. The preparation method according to claim 4, It is characterized in that The inert atmosphere includes nitrogen atmosphere, argon atmosphere or helium atmosphere; the calcination temperature is 500-700° C. and the calcination time is 1-6 hours.

9. The preparation method according to claim 4, It is characterized in that The reducing atmosphere includes a hydrogen atmosphere; the reducing temperature is 500 to 700° C., and the reducing time is 1 to 6 hours.

10. Use of the silicon nitride-supported metal nanoparticle composite material according to any one of claims 1 to 3 or the silicon nitride-supported metal nanoparticle composite material prepared by the preparation method according to any one of claims 4 to 9 as a catalyst in the decomposition of ammonia to produce hydrogen.

Citation Information

Patent Citations

  • High-dispersion transition metal catalyst anchored to silicon nitride and preparation method and application thereof

    CN114433246A

  • Low-temperature efficient ammonia decomposition catalyst and preparation method thereof

    CN115945212A

  • Process for the thermal decomposition of ammonia and reactor for carrying out said process

    US20180230006A1

  • Systems and methods for processing ammonia

    WO2024107776A1

Cited By

  • Method for producing hydrogen through ammonia decomposition based on cerium dioxide reverse catalyst

    CN121513890A

  • A method for hydrogen production by ammonia decomposition based on ceria reverse phase catalyst