Machining method for casting barrel opening type framework
By processing the process bosses on both sides of the blank of the cylinder frame and casting them based on it, the problem of structural deformation of the cylinder frame during the casting process is solved, and a higher quality and efficiency molding is achieved.
Patent Information
- Application Number
- CN202411181254.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing cylinder frame is prone to structural deformation during casting, resulting in inaccurate positioning and further aggravate the structural deformation problem of the final product, especially in the case of large thin-walled cylinders.
Using the machining method of casting cylinder open skeleton, the positioning reference is provided by processing the process boss on both sides of the blank, and rough milling and fine milling are carried out based on the process boss to form a semi-completion piece, and then artificial aging is performed. and fine milling in batches to gradually reduce the processing allowance and avoid structural deformation.
It effectively reduces the deformation of the final formed product, improves product quality and processing efficiency, and ensures accurate positioning and precise molding of the structure.
Smart Images

Figure CN118905574A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of mechanical processing technology, and in particular relates to a processing method for a casting cylinder open-type skeleton. Background Art
[0002] As a structural element, the cylinder usually refers to a structure with a cylindrical shape composed of multiple parts or components, and the skeleton serves as the basis to provide support for the cylinder, so that the cylinder can be combined into the final cylindrical structure. This structure can not only withstand the vertical gravity load, but also effectively transmit and disperse the horizontal force. It has a wide range of applications in many fields.
[0003] Cylinder frame castings have their unique advantages, especially investment castings, which can be arbitrarily complex in shape and can be integrally formed with almost no or even no allowance. Their performance and reliability are comparable to those of plastic deformation components, and their manufacturing cost and production cycle are significantly better than those of plastic deformation components.
[0004] However, once the size of the existing cylinder skeleton is larger than a certain value and the thickness is thin, such as a large thin-walled cylinder, the size is generally in the range of 1200mm to 1500mm in length, 400mm to 600mm in width, 350mm to 500mm in height, and the wall thickness is generally in the range of 2mm to 4mm. During casting, structural deformation is prone to occur. At the same time, deformation will cause inaccurate positioning of the cylinder skeleton, which will further aggravate the problem of structural deformation of the final product. Summary of the invention
[0005] The present application aims to solve the technical problem of deformation of the cylinder frame structure at least to a certain extent. To this end, the present application provides a processing method for a cast cylinder open frame, which can quickly position the structure and avoid deformation of the structure during casting, thereby reducing the deformation of the final molded product, improving product quality, and at the same time improving processing efficiency.
[0006] The embodiment of the present application provides a method for processing a casting cylinder open frame, the cylinder open frame comprises a main body, a plurality of arched frames and a plurality of process bosses, one side of the main body is provided with an open groove extending from one end to the other end, the plurality of arched frames are arranged at intervals from one end to the other end of the main body, the two ends of the arched frames are connected to the relative positions of the open groove of the main body, the plurality of process bosses are connected to the main body at intervals and are located at the edge of the open groove, the processing method comprises:
[0007] Place the blank of the cylindrical open frame on the work surface, level it through the side and two end faces of the blank, and draw the outline;
[0008] Fix the blank so that its opening groove faces upward, roughly mill out the process bosses on both sides of the blank and then fine mill the process bosses;
[0009] Use the process boss as a reference to calibrate and fix the blank, and perform rough milling on the outer and inner contours of the blank, leaving a 2mm±0.1mm margin;
[0010] In the free state, the contour and deformation of the blank are tested, and artificial aging is performed to form a semi-finished part;
[0011] The semi-finished part is corrected and fixed based on the process boss, and the outer contour of the semi-finished part is roughly milled, leaving a 1mm±0.1mm margin;
[0012] The semi-finished part is corrected and fixed based on the process boss, and the inner and outer contours of the semi-finished part are fine-milled for multiple times, leaving allowances in turn, and the allowances are gradually reduced to zero.
[0013] In an optional embodiment, rough milling of the outer contour and the inner contour of the blank includes:
[0014] Fix the blank upside down with the open slot facing downward, use the process boss as a reference for calibration, and then roughly mill the outer contour of the blank;
[0015] Fix the blank with the open groove facing upward, use the side of the process boss as a reference for correction, and then roughly mill out the inner contour of the blank in the open groove.
[0016] In an optional embodiment, the rough milling and fine milling process bosses include the following steps:
[0017] Fill the gap between the blank and the work surface, fix it after coordinating the processing allowance, roughly mill out multiple process bosses, and drill process holes;
[0018] The outer contour of the blank is measured at a fixed point to obtain the xyz coordinates, and the measured data is compared with the theoretical model. At the corresponding deviation between the measured data and the theoretical model, the blank is adjusted for alignment;
[0019] Through the machine tool dotting method, the xyz coordinates of each part of the outer contour of the blank are made consistent with the theoretical model;
[0020] Carry out finish milling on the technological boss.
[0021] In an optional embodiment, when rough milling the outer contour of the blank, the following steps are included:
[0022] The two end faces of the blank are used as reference for calibration to ensure that the deviation between the outer contour of the blank and the theoretical model is less than or equal to 0.2 mm;
[0023] The outer contour of the blank is rough milled, and the outer contour includes the convex surface, two end faces and two side faces of the blank.
[0024] In an optional embodiment, rough milling the inner contour of the blank includes the following steps:
[0025] The machine tool's y-axis is corrected by the side of the process boss, and the machine tool's y-axis is divided into data points on the sides of multiple process bosses;
[0026] Correction is performed through the plane of the process boss, and the x-axis of the machine tool takes data from the two end faces of the blank;
[0027] Fix the blank and rough mill its inner contour.
[0028] In an optional embodiment, when finishing the outer contour or inner contour of the semi-finished part, the following steps are included:
[0029] Clamp and fix the semi-finished component and align it so that the opening slot faces downward; or fix and align the semi-finished component so that the opening slot faces upward;
[0030] The outer contour or the inside of the semi-finished part is fine-milled in n times, with allowances reserved from 1 to n-1 times, and the allowances are gradually reduced in each time.
[0031] In an optional implementation manner, when fine milling the outer contour of the semi-finished component, the convex surface, the two sides and the end surface are processed in sequence.
[0032] In an optional embodiment, it also includes:
[0033] Milling process bosses make the outer contour of the semi-finished part transition smoothly;
[0034] The milling position is fine-milled at least twice, with an allowance reserved before the last time and the allowance gradually reduced, and finally fine-milled to the corresponding size of the model.
[0035] In an optional embodiment, when fixing the blank or semi-finished part, the arched frame is never subjected to force; if the opening slot faces downward, a clamp is placed on the work surface, and the process boss is fixed to the clamp so that the arched frame is spaced apart from the clamp.
[0036] In an optional embodiment, it also includes: when the cylindrical open-type skeleton is in a free state, detecting the contour and deformation of the cylindrical open-type skeleton, if the contour of the cylindrical open-type skeleton deviates from the model, performing fine milling on the deviated portion to form the cylindrical open-type skeleton.
[0037] It can be seen from the above technical solution that the beneficial effects of this application are:
[0038] The present application processes process bosses on both sides of the blank first to provide a reference for subsequent processing, and then fine-mills the process bosses to ensure subsequent positioning accuracy, and then fixes the blank with the process boss position reference to complete the rough milling of the outer contour and the inner contour, and preliminarily form the outer and inner shapes corresponding to the theoretical model, and then forms a semi-finished product through artificial aging. Since the process bosses are located on both sides of the blank and are distributed in multiples, other parts of the blank are never in contact with the work surface or other fixing tools. Therefore, during the processing, the force on other parts of the blank is avoided during the processing, such as the arched frame is not in contact with the force, which significantly reduces the impact on the blank. The impact of the blank; then, the outer contour and inner contour of the semi-finished part are fine-milled based on the process boss. The process boss can not only quickly and accurately position the semi-finished part, but also reduce the impact on the overall structure during the fine milling process. Through multiple fine milling, the force of the milling tool on the semi-finished part each time can be controlled within a smaller range, and the milling amount each time is small, the temperature can be controlled and will not be too high, further reducing the impact of processing on the overall structure. In this way, the present application can quickly position the structure, avoid deformation of the structure during casting, reduce the deformation of the final molded product, improve product quality, and at the same time improve processing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions in the embodiments of the present application, a brief introduction will be given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other embodiments and drawings can be obtained based on these drawings without creative work.
[0040] Figure 1 A schematic diagram of an embodiment of the cylindrical open-type skeleton of the present invention is shown;
[0041] Figure 2 A schematic diagram of an embodiment of step S1 of a method for processing a casting cylinder open frame of the present invention is shown;
[0042] Figure 3 A schematic diagram of an embodiment of step S3 or S5 of a method for processing a cast cylindrical open frame of the present invention is shown;
[0043] Figure 4 A schematic diagram of an embodiment of step S4 of a method for processing a cast cylindrical open frame according to the present invention is shown;
[0044] Figure 5 A schematic diagram of an embodiment of step S6 of a method for processing a cast cylindrical open frame according to the present invention is shown;
[0045] Figure 6 A schematic diagram of an embodiment of step S7 of a method for processing a cast cylindrical open frame according to the present invention is shown;
[0046] Figure numerals: 10, cylindrical open frame; 11, main body; 12, arched frame; 13, process boss; 14, open groove; 20, work surface; 30, tooling; 40, pressing block; 50, fixture; 51, support block. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] It should be noted that all directional indications in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between various components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0049] In the present invention, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0050] In addition, in the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0051] The present application is described below with reference to the accompanying drawings and specific embodiments:
[0052] Please refer to Figure 1The first embodiment of the present application provides a method for processing a cast cylindrical open-type skeleton. The cylindrical open-type skeleton 10 includes a main body 11, a plurality of arched skeletons 12 and a plurality of process bosses 13. The cylindrical open-type skeleton 10 can be made of titanium alloy, or aluminum alloy or other alloys. The present method is more suitable for processing cylindrical skeletons made of high-strength materials. One side of the main body 11 is provided with an open groove 14 extending from one end to the other end. As shown in the figure, one side of the top surface of the main body 11 is provided with an open groove 14. A plurality of arch frames 12 are arranged at intervals from one end to the other end of the main body 11. For example, 4 arch frames 12 are provided, or other numbers of at least two may be provided. The arch frames 12 are arched, and may be a semicircular shape or a part of a circle. Both ends of the arch frames 12 are connected to the relative positions of the opening groove 14 of the main body 11. As shown in the figure, the arch frames 12 span the opening groove 14 and protrude from the top surface of the main body 11. The arch frames 12 may be integrally formed with the main body 11, or may be fixed with screws or bolts. A plurality of process bosses 13 are connected to the main body 11 at intervals and are located at the edges of the opening groove 14. The number of the process bosses 13 is 10-20, such as 7 pairs of 14 process bosses 13 are symmetrically provided on both sides of the main body 11. During processing, a machine tool with a rough milling tool and a fine milling tool is used. The milling operation is performed through the tool. The program path can be set before the operation. The machine tool processing is an existing technology. The processing methods include:
[0053] Please refer to Figure 2 S1. Place the blank of the cylindrical open-type skeleton 10 on the work surface 20, level the side and both end faces of the blank, and draw the contour line; before placing the blank, first perform conventional size detection of the casting blank and detect the distribution of the blank allowance to ensure that it meets the processing standards; when placing the blank, align the side of the blank to ensure that the process boss 13 to be processed is located on the same plane during subsequent casting, and then level the end faces at both ends of the main body 11, and finally confirm the position of the characteristic boss inside the open groove 14, and ensure that the alignment error is less than or equal to 0.2mm before drawing the contour line; when drawing the contour line, use the tool of the machine tool to carve it, or use other conventional methods to carve it, or use the fitter to draw the line, according to the rough step and evenly distribute the allowance of the product design drawing, draw the contour line, and determine the position to be processed.
[0054] S2, fix the blank so that its open groove 14 faces upward, roughly mill out the process boss 13 on both sides of the blank and then finely mill the process boss 13; when fixing the blank, the tooling 30 and the pressing block 40 can be used for fixing, the tooling 30 can be an existing free-standing tooling 30, the top surface of the tooling 30 serves as the work table 20, and the two ends or both sides of the tooling 30 are fixed with chucks, the chucks have threaded holes and can be fixed to the tooling 30 by screws, so that it is convenient to fix the blank on the work table 20, at this time, the open groove 14 faces upward, and the arched skeleton 12 is located above the main body 11; when fixing the blank, the gap surface between the bottom of the blank and the work table 20 is padded, and at least A pressing block 40 presses the blank to fix it. The pressing block 40 is in a block shape and is equipped with screws. If the main body 11 has a hole or an opening running through the top and bottom, the pressing block 40 can be placed at the hole or the opening, and then the pressing block 40 is fixed to the main body 11 with screws, thereby achieving the fixation of the main body 11. The expected flatness of the process boss 13 is remeasured online, and after coordinating the machining allowance, 14 process bosses 13 are milled out on the edges of the opening groove 14 on both sides of the main body 11. The process boss is a block protruding from the side of the main body 11. The upper surface of the process boss 13 is roughly milled, leveled according to the model, and a process hole is drilled. The process hole is a threaded hole, and then the process boss 13 is finely milled to ensure the machining accuracy of the upper surface and the side.
[0055] Please refer to Figure 3 S3, calibrate and fix the blank with the process boss 13 as the reference, and roughly mill the outer contour and inner contour of the blank, leaving a 2mm±0.1mm margin; control the machining margin at 2mm±0.1mm; during rough milling, fix the blank on the work table 20, fix it with the tooling 30, or fix it with the fixture 50. After fixation, recheck the dimensions of the outer contour at various locations. Multiple measuring points can be set, and the actual coordinate values of each measuring point are measured by the machine tool, and compared with the values of the theoretical model; check the uniformity of the blank margin, and roughly mill the convex surface and both end surfaces of the blank. The convex surface is the side opposite to the arched skeleton 12, which is the top surface of the blank when the opening groove 14 of the blank faces downward. Avoid the pressing block 40 during rough milling, and reserve a 2mm margin on the single side of the main body 11 to ensure that 90% of the area can be exposed to light and the overall metallic luster.
[0056] Please refer to Figure 4S4, in a free state, detect the contour and deformation of the blank, and perform artificial aging to form a semi-finished product; in the above process, the blank is fixed, and the fixed state is released at this time, such as removing the above-mentioned pressing block 40 and the above-mentioned chuck, so that the blank is only placed on the workbench 20 without restriction. At this time, the outer contour of the blank is detected again, and the deformation is detected to ensure that the difference between the coordinate values of each measuring point of the blank and the coordinate value of the theoretical model is within the error range; then the blank is artificially aged, which refers to the operation of maintaining a certain temperature above room temperature for a certain period of time to improve its mechanical properties. Artificial aging can shorten the processing time by controlling factors such as heating temperature and holding time, eliminate or reduce the micro stress and machining residual stress in the steel after quenching, and prevent deformation and cracking. This process is a prior art.
[0057] Please refer to Figure 3 S5. Use the process boss 13 as a reference to calibrate and fix the semi-finished part, and perform rough milling on the outer contour of the obtained semi-finished part, leaving a 1mm±0.1mm margin; connect the process boss 13 with the support block 51, and the support block 51 is connected to the fixture 50, such as using screws to pass through the process holes to connect and fix each process boss 13 with the corresponding support block 51. Since each support block 51 is pre-designed, the top surface of each support block 51 is located on the same plane, so that the correction and fixation of the semi-finished part are completed, and the outer contour of the semi-finished part is rough milled, and the machining allowance is controlled at 1mm to ensure uniform reservation. Use a rough milling tool to rough mill the convex surface, two end faces and side edges, so as to complete the secondary rough milling of the outer contour, avoiding the process boss 13, the pressure block 40 and the chuck during rough milling.
[0058] Please refer to Figure 5 , S6, calibrate and fix the semi-finished part with the process boss 13 as the reference, and perform fine milling on the inner and outer contours of the obtained semi-finished part in multiple times, leaving allowances in turn, and the allowances are gradually reduced to zero, and the inner and outer contours are respectively fine milled at least twice, which requires fine milling in two different fixing processes. Specifically, fix the semi-finished part on the work table 20 in the above manner, with the open groove 14 facing upward, and perform fine milling on the inner contour; or invert the semi-finished part, fix the semi-finished part on the support block 51 of the fixture 50, with the open groove 14 facing downward, and perform fine milling on the outer contour. During fine milling, the machining allowance is controlled at 0.3±0.05mm for the first time, and then gradually reduced each time. The last time, no allowance is left and the part is directly processed in place, and finally formed.
[0059] Please refer to Figure 6S7, when the cylindrical open-type skeleton 10 is in a free state, detect the contour and deformation of the cylindrical open-type skeleton 10, that is, in the same way as in the above step S4, release the fixed state so that the cylindrical open-type skeleton 10 is not restricted. If the contour of the cylindrical open-type skeleton 10 deviates from the model, that is, the coordinates of the measuring point and the coordinates of the corresponding point of the model deviate, then the deviated part is finely milled, which mainly includes deburring and finishing to form the cylindrical open-type skeleton 10, and finally the size is fully detected.
[0060] The existing technology of cylindrical skeleton processing is prone to structural deformation. At the same time, deformation will cause inaccurate positioning of the cylindrical skeleton, which will further aggravate the problem of structural deformation of the final product. This is mainly caused by the structure of the cylindrical skeleton: (1) The cylindrical skeleton has a large aspect ratio, a grid structure, thin walls, and weak rigidity; (2) The cylindrical skeleton has many dimensional coordination relationships. In the casting process of the cylindrical skeleton, there are also the following reasons: First, the elastic modulus of the part material is low, which causes it to produce a large rebound after deformation under load, causing the structural parts to deviate from the tool during machining; second, the chemical activity of the part material is high and the affinity is large. When the cutting temperature is high, the cutting and cut surfaces bite with the tool material to produce a more serious sticking phenomenon, causing severe adhesion and wear of the tool. Especially for large cylindrical skeletons with thin walls, this causes the problem of easy deformation of the skeleton structure during production.
[0061] For the skeleton corresponding to the large thin-walled cylinder, the present application can solve the above-mentioned deformation problem. The size of the large thin-walled cylinder is generally in the range of 1200mm to 1500mm in length, 400mm to 600mm in width, and 350mm to 500mm in height. The wall thickness is generally in the range of 2mm to 4mm, including the endpoint values. The present application first processes the process boss 13 on both sides of the blank to provide a reference for subsequent processing, and then fine-mills the process boss 13 to ensure the subsequent positioning accuracy. The blank is then fixed with the process boss 13 as the reference, and the rough milling of the outer and inner contours is completed to preliminarily form the outer and inner shapes corresponding to the theoretical model, and then artificial aging is performed to form a semi-finished part. Since the process boss 13 is located on both sides of the blank and is distributed in multiples, the other parts of the blank are always not in contact with the work table 20 or other When the fixed tools are in contact with each other, the force on other parts of the blank during processing is avoided, such as the arched frame 12 is not in contact with the force, which significantly reduces the impact on the blank; then the outer contour and inner contour of the semi-finished part are fine-milled based on the process boss 13. The process boss 13 can not only quickly and accurately position the semi-finished part, but also reduce the impact on the overall structure during fine milling. Through multiple fine milling, the force of the milling tool on the semi-finished part each time can be controlled within a smaller range, and the milling amount each time is small, the temperature can be controlled and will not be too high, further reducing the impact of processing on the overall structure. In this way, the present application can quickly position the structure, avoid deformation of the structure during casting, reduce the deformation of the final molded product, improve product quality, and at the same time improve processing efficiency.
[0062] In an optional embodiment, when rough milling the outer contour and inner contour of the blank, it includes: fixing the blank upside down with the opening groove 14 facing downward, calibrating with the process boss 13 as a reference, fixing each process boss 13 on the corresponding support block 51, and then rough milling the outer contour of the blank. The pressure block 40 can be used to fix the process boss 13 and the inner wall of the main body 11; fixing the blank with the opening groove 14 facing upward, calibrating with the side of the process boss 13 as a reference, making the side of each process boss 13 consistent with the positioning point of the machine tool, and then rough milling the inner contour of the blank in the opening groove 14. The above outer contour includes the convex surface, two end faces and two side faces of the blank, and the above inner contour is the internal shape of the main body 11 at the opening groove 14, including the inner profile, rib groove, groove, reinforcing rib and characteristic boss. The characteristic boss is used as the reference for positioning. During rough milling, the inner contour is smoothed to ensure the flatness of the inner profile, rib groove and groove. Note that when processing the inner contour in rough milling or subsequent fine milling, the pressing block 40 is removed. When the above correction is performed, the x-axis data of the reading in the machine tool data is taken from the end faces of the two ends of the main body 11 as the reference, and the y-axis data is taken from the side of the process boss 13 as the reference.
[0063] In an optional embodiment, the rough milling and fine milling process boss 13 includes the following steps:
[0064] The gap between the blank and the worktable 20 is filled, and the machining allowance is coordinated before fixing. Coordination refers to the process of alignment to ensure that all the rough-milled places have machining allowances. Along the two sides of the product structure, a plurality of process bosses 13 are roughly milled on the edges of the opening groove 14 and on both sides of the main body 11, such as 7 groups of 14 in total, and process holes are drilled on the process bosses 13. The process holes can be threaded holes that pass through the two sides of the process bosses 13; the outer contour of the blank is measured at a fixed point, and each point is a measurement point predetermined by the machine tool. The xyz coordinates of each measurement point are obtained, and the measurement data are compared with the theoretical model, that is, the measurement point The coordinates are compared with the coordinates of the corresponding points of the theoretical model to find out the deviation, and the blank is adjusted for alignment at the corresponding places where the deviations between the measured data and the theoretical model; the xyz coordinates of the outer contour of the blank are made consistent with the theoretical model through machine tool dotting, specifically referring to the coordinates of each measuring point and the coordinates of the corresponding points of the theoretical model, to ensure that there is no deviation and allow a certain error; the process boss 13 is fine-milled, and the fine-milling process needs to process the shape of the process boss 13 so that the top surfaces of the process boss 13 are on the same plane, and the side edges of the process boss 13 on both sides are respectively on the same straight line.
[0065] In an optional embodiment, when rough milling the outer contour of the blank, the following steps are included: the two end faces of the blank are used as references for correction to ensure that the deviation value between the outer contour of the blank and the theoretical model is less than or equal to 0.2 mm; that is, the two end faces of the blank and each process boss 13 are used as references for correction. The outer contour of the blank is rough milled, and the outer contour includes the convex surface, the two end faces and the two side faces of the blank, which can be rough milled separately in no particular order. In an optional embodiment, when rough milling the inner contour of the blank, the following steps are included: calibrating through the side of the process boss 13, the y-axis of the machine tool takes numbers at the center of the sides of multiple process bosses 13; calibrating through the plane of the process boss 13, the x-axis of the machine tool takes numbers at the center of the two end faces of the blank; taking numbers at the center is a method commonly used in the milling process of the machine tool, which involves the correspondence between the machine tool coordinate system and the workpiece coordinate system, and accurately determining the position of the workpiece in the machine tool; fixing the blank and rough milling its inner contour, that is, rough milling the above-mentioned inner profile, rib grooves, etc., reserving processing allowances, and preliminarily processing the internal shape of the main body 11.
[0066] In an optional embodiment, when finishing the outer contour or inner contour of the semi-finished part, the following steps are included:
[0067] The semi-finished part is clamped and corrected so that the opening groove 14 faces downward. The operation in the rough milling process is also adopted. The semi-finished part is fixed by a clamp 50 and a support block 51, and the correction is performed through the contact surface between the process boss 13 and the support block 51; or the semi-finished part is fixed and corrected so that the opening groove 14 faces upward. The tooling 30 is also adopted, and the two ends or both sides of the semi-finished part are fixed by a chuck; the outer contour or the inner part of the semi-finished part is fine-milled n times, wherein 1 to n-1 times reserve a margin, and the margin is gradually reduced with each time. For example, fine milling is performed in 2 times. When fine milling the outer contour, the opening groove 14 is fixed downward, and when fine milling the inner contour, the opening groove 14 is fixed upward. When fine milling the outer contour of the semi-finished part, the processing is performed in the order of the convex surface, the two sides and the end face.
[0068] In an optional implementation manner, the method further includes, after performing step S6:
[0069] Milling process boss 13 makes the outer contour of the semi-finished product transition smoothly. The process boss 13 is designed by this method. After finishing the fine milling, the process boss 13 needs to be removed, and the opening groove 14 is facing upward. The semi-finished product after fine milling is fixed by the above-mentioned tooling 30, and each process boss 13 is milled to ensure a smooth transition of the milling position and a smooth outer contour of the product; the milling position is fine milled at least twice, and a margin is reserved before the last time and the margin is gradually reduced. For example, each milling position is fine milled to form a semi-fine arc surface, leaving a margin of 0.2mm, and then a second fine milling is performed, and finally the fine milling is performed to the corresponding size of the model. Please refer to Figure 5 After removing the process boss 13, step S7 is required to perform fine milling on the deviated part, including deburring and finishing. At this time, the cylindrical open-type skeleton 10 is inverted and a free-standing tooling is used. The top surface of the tooling is a work surface 20. A supporting connecting plate is installed on the work surface 20. The top of the supporting connecting plate can be set to a flat plate shape. The tops of multiple supporting connecting plates are just in close contact with the inner contour surface of the main body 11. In this way, the cylindrical open-type skeleton 11 is fixed and supported by multiple supporting connecting plates, which is convenient for the processing of this step.
[0070] In an optional embodiment, when fixing a blank or a semi-finished part, the arched frame 12 is always free from stress; if the opening slot 14 faces downward, a clamp 50 is placed on the work surface 20, and the process boss 13 is fixed to the clamp 50, so that the arched frame 12 is spaced from the clamp 50. As shown in the figure, a clamp 50 is used, and the top surface of the clamp 50 is used as the work surface 20. The clamp 50 is provided with support blocks 51. There are 14 support blocks 51 in total, and the top surfaces are all located on the same plane, and the positions correspond to the 14 process bosses 13 respectively. The support blocks 51 are welded to the work surface 20, and threaded holes are opened on the tops of the support blocks 51. When fixing a blank or a semi-finished part, the process boss 13 can be aligned with each support block 51, and each process boss 13 can be fixed to the corresponding support block 51 by screws through the process holes, so that the precise positioning of the structure is completed, and at this time, the arched frame 12 is in contact with the support blocks 51 and is also free from stress. Another form of support block 51 may be provided, which is connected to the middle of the fixture 50, and a plurality of support blocks 51 are arranged at intervals so that when the opening slot 14 faces downward, the top surface of the support block 51 can be supported on the inner contour of the blank or semi-finished part.
[0071] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", "optional example" or "optional implementation" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0072] In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the fact that they can be implemented by ordinary technicians in this field. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0073] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A method for processing a cast cylindrical open frame, characterized in that: The cylindrical open-type skeleton comprises a main body (11), a plurality of arched skeletons (12) and a plurality of process bosses (13); one side of the main body (11) is provided with an open groove (14) extending from one end to the other end; the plurality of arched skeletons (12) are arranged at intervals from one end to the other end of the main body (11); the two ends of the arched skeleton (12) are connected to the relative positions of the open groove (14) of the main body (11); the plurality of process bosses (13) are connected to the main body (11) at intervals and are located at the edge of the open groove (14); and the processing method comprises: Placing the blank of the cylindrical open frame on a work surface (20), leveling the side edges and two end faces of the blank, and drawing contour lines; Fixing the blank so that the opening groove (14) faces upward, roughly milling out process bosses (13) on both sides of the blank and then fine milling; The blank is corrected and fixed with the process boss (13) as a reference, and the outer contour and inner contour of the blank are roughly milled, leaving a margin of 2 mm ± 0.1 mm; In a free state, the contour and deformation of the blank are detected, and artificial aging is performed to form a semi-finished part; The semi-finished part is corrected and fixed based on the process boss (13), and the outer contour of the semi-finished part is roughly milled, leaving a margin of 1 mm ± 0.1 mm; The semi-finished part is corrected and fixed with the process boss (13) as a reference, and the inner contour and outer contour of the semi-finished part are finely milled for multiple times, leaving allowances in turn, and the allowances are gradually reduced to zero.
2. The method for processing a casting cylinder open frame according to claim 1, characterized in that: When the outer contour and the inner contour of the blank are roughly milled, it includes: Fix the blank upside down so that the opening groove (14) faces downward, calibrate it with the process boss (13) as a reference, and then roughly mill the outer contour of the blank; The blank is fixed so that the opening groove (14) faces upward, and the side edge of the process boss (13) is used as a reference for correction, and then the inner contour of the blank in the opening groove (14) is roughly milled.
3. The method for processing the open-type casting cylinder frame according to claim 2, characterized in that: The rough milling and fine milling of the process boss (13) include the following steps: Filling the gap between the blank and the work surface (20), fixing after adjusting the machining allowance, roughly milling out a plurality of process bosses (13), and drilling process holes; The outer contour of the blank is measured at a fixed point to obtain xyz coordinates, and the measured data is compared with the theoretical model, and the blank is adjusted for alignment at the corresponding deviation between the measured data and the theoretical model; Through the machine tool dotting method, the xyz coordinates of each location of the outer contour of the blank are made consistent with the theoretical model; The process boss (13) is subjected to precision milling.
4. The method for processing a casting cylinder open frame according to claim 2, characterized in that: When rough milling the outer contour of the blank, the following steps are included: The two end faces of the blank are used as references for calibration to ensure that the deviation between the outer contour of the blank and the theoretical model is less than or equal to 0.2 mm; The outer contour of the blank is subjected to rough milling, and the outer contour includes a convex surface, two end surfaces and two side surfaces of the blank.
5. The method for processing the open-type casting cylinder frame according to claim 2, characterized in that: When rough milling the inner contour of the blank, the following steps are included: Calibration is performed through the side of the process boss (13), and the y-axis of the machine tool takes data from the side of multiple process bosses (13); Correction is performed through the plane of the process boss (13), and the x-axis of the machine tool takes data from the two end surfaces of the blank; The blank is fixed and its inner contour is roughly milled.
6. The method for processing a casting cylinder open frame according to claim 1, characterized in that: The fine milling of the outer contour or inner contour of the semi-finished part includes the following steps: The semi-finished component is clamped, fixed and corrected so that the opening slot (14) faces downward; or the semi-finished component is fixed and corrected so that the opening slot (14) faces upward; The outer contour or the interior of the cylindrical open-type skeleton is finely milled n times, wherein margins are reserved from 1 to n-1 times, and the margins are gradually reduced in each time.
7. The method for processing a casting cylinder open frame according to claim 6, characterized in that: When fine milling the outer contour of the semi-finished part, the processing is carried out in the order of the convex surface, the two sides and the end face.
8. The method for processing a casting cylinder open frame according to any one of claims 1 to 7, characterized in that: Also includes: Milling the process boss (13) to make the outer contour of the semi-finished part transition smoothly; The milling position is fine-milled at least twice, with an allowance reserved before the last time and the allowance gradually reduced, and finally fine-milled to the corresponding size of the model.
9. The method for processing a casting cylinder open frame according to claim 1, characterized in that: When the blank or the semi-finished product is fixed, the arched frame (12) is always free from stress; if the opening groove (14) faces downward, a clamp (50) is placed on the work surface (20), and the process boss (13) is fixed to the clamp (50) so that the arched frame (12) and the clamp (50) are spaced apart.
10. The method for processing a casting cylinder open frame according to claim 1, characterized in that: Also includes: When the cylindrical open-type skeleton is in a free state, the contour and deformation of the cylindrical open-type skeleton are detected. If the contour of the cylindrical open-type skeleton deviates from the model, fine milling is performed on the deviated portion to form the cylindrical open-type skeleton.
Citation Information
Patent Citations
Vaulted thin-wall part machining method
CN108705102A
Nuclear power station containment steel lining thin shell type hemispherical dome structure and manufacturing method thereof
CN115846827A
Method for machining hollow thin-wall framework part with multi-angle composite surface structure
CN115922250A
Machining process for large-diameter thin-walled part
WO2020253818A1
Inspection method for friction stir welded part, and welding device
WO2022210248A1
Cited By
Square open end frame type thin-wall part and machining method
CN119820005A