Manufacturing method of shunt ring of collector ring device
By employing processes such as drawing, upsetting forging, low-temperature rolling, and cold bending, combined with forming mold design, the problems of material consumption, time consumption, and uneven strength in the manufacturing of splitter rings have been solved, achieving efficient and stable production of splitter rings.
Patent Information
- Application Number
- CN202411419627.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for manufacturing shunt rings are material-intensive and time-consuming, making it difficult to meet design requirements. Furthermore, the product strength is uneven, affecting its service life.
The current distribution ring of the collector ring device is prepared by using the processes of drawing, upsetting forging, low temperature rolling and cold bending forming, combined with the design of forming mold.
It reduces raw material consumption, shortens processing time, improves product strength and consistency, extends service life, and is suitable for mass production.
Smart Images

Figure CN118905580A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electromechanics, and in particular to a method for manufacturing a shunt ring of a collector ring device. Background Art
[0002] Collector rings, also known as slip rings, are generally used in high-performance, high-precision equipment. They are of great help to the rotation of high-end industrial electrical equipment and precision electrical equipment. They are often used in aerospace equipment, automatic processing equipment, mining equipment, medical equipment, radar equipment, etc. Slip rings provide these devices with reliable energy signal transmission solutions, thereby achieving more complex movements. Among them, the function of the shunt ring in the slip ring rotor is to extract the current generated by the rotor and evenly distribute it to the slip ring, so as to avoid the high current voltage output being blocked, resulting in reduced efficiency, or even high temperature and high voltage damage to the equipment.
[0003] There are two main methods for manufacturing the splitter ring: Forged into a ring shape, and then machined into shape. However, due to the thin wall thickness of the product structure, the forged ring needs to increase the packaging capacity, resulting in greater material loss; during machining, the thin wall thickness causes greater deformation, the product size is difficult to control, and the processing difficulty increases; directly using wire cutting will have a longer processing cycle.
[0004] The upper and lower half rings are forged into strips and then processed to product specifications, and then heated by a flame gun and bent by hammering. This method can save materials, but the forgings are thin and easy to deform, and the processing is difficult. After the material is over-fired at high temperature, its overall strength properties are reduced, the internal quality is uneven, and it cannot meet the design strength requirements, which affects the service life of the product.
[0005] The above two methods both have certain defects, consume materials and are time-consuming, and are difficult to meet design requirements. Summary of the invention
[0006] In view of the above-mentioned shortcomings that currently exist, the present invention provides a manufacturing method for a shunt ring of a collector ring device, which can effectively reduce consumables and shorten the processing time, and can also maximize the integrity of the metal streamlines inside the original forging and the retention amount on the heat treatment surface, so that the product has higher strength performance and extends the product's service life.
[0007] To achieve the above object, the embodiments of the present invention adopt the following technical solutions: A method for manufacturing a shunt ring of a collector ring device, characterized in that the method for manufacturing a shunt ring of a collector ring device comprises: Selecting raw materials and performing stretching, upsetting and forging on the raw materials to obtain blanks; The blank is subjected to low temperature rolling to obtain a plate, specifically, the blank is heated to 300-350°C, kept warm for 1-2 hours, and then rolled to obtain a plate; The plate is cut according to the size of the diverter ring and subjected to solution heat treatment to obtain the cut material; The sheared materials are cold-bent by using forming dies to obtain bent parts; The bent part is machined to obtain a diverter ring.
[0008] According to one aspect of the present invention, the raw material is selected and stretched and upset forged to obtain the blank, specifically, the selected raw material is heated to 650-850°C, the raw material is stretched and upset, and after the last upsetting, the raw material is rounded to obtain the initial forging.
[0009] According to one aspect of the present invention, the raw material is a chromium-zirconium-copper material, wherein Zr: 0.05-0.25%, Cr: 0.50-1.50%, and Cu+Cr+Zr≥99.7%.
[0010] According to one aspect of the present invention, the blank is subjected to low temperature rolling to obtain a plate, specifically: the low temperature rolling is performed multiple times, and the deformation amount of each rolling is controlled to be 3mm~5mm.
[0011] According to one aspect of the present invention, the forming mold includes an upper half ring forming mold and a lower half ring forming mold, the upper half ring forming mold includes an upper half ring upper mold, a core mold and an upper half ring lower mold, and the lower half ring forming mold includes a lower half ring upper mold and a lower half ring lower mold.
[0012] According to one aspect of the present invention, the core mold has a 255° arc surface.
[0013] According to one aspect of the present invention, the rolling range of the plate is 5mm-50mm, and the cold bending range of the sheared material is R50mm-R500mm.
[0014] According to one aspect of the present invention, the method of cold-bending the sheared materials using forming dies to obtain bent parts includes: bending the sheared materials using an upper semi-ring forming die; and bending the sheared materials using a lower semi-ring forming die.
[0015] According to one aspect of the present invention, the bending process of the sheared material by the upper half-ring forming mold includes: placing the sheared material between the core mold and the upper half-ring lower mold and dividing the length evenly; applying pressure along the pressure direction by a pressure device to bend the sheared material to close the mold; separating the upper half-ring upper mold and the core mold to obtain a bent part.
[0016] According to one aspect of the present invention, the sheared material is bent by a lower half-ring forming mold, including: placing the sheared material between the lower half-ring upper mold and the lower half-ring lower mold and dividing the length evenly; applying pressure along the pressure direction by a pressure device to bend the sheared material until the mold is closed; separating the lower half-ring upper mold and the lower half-ring lower mold to obtain a bent part.
[0017] Advantages of the present invention: (1) The combined forging, rolling and cold bending forming process is adopted, which greatly improves the utilization rate of raw materials, reduces energy consumption and shortens the processing cycle.
[0018] (2) Rolling forgings at low temperatures deforms the material to enhance the density of the structure and increase the strength margin, making full preparations for subsequent solution aging heat treatment. (3) The forming mold adopts a modular design, the product shape is uniform, the size deviation is small, the interchangeability is strong, it is convenient and fast, and it is easy to mass produce, saving a lot of time for finished product processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 It is a structural schematic diagram of the present invention; Figure 2 is a flow chart of the present invention; Figure 3 It is a schematic diagram of forming a preliminary forging obtained by forging a blank according to a preset forging process according to the present invention; Figure 4 It is a flow chart of forging a steel ingot to obtain a preliminary forging according to the forging process and die of the present invention; Figure 5 It is the heat treatment process curve diagram of the present invention; Figure 6 It is a structural schematic diagram of the upper half ring tooling of the present invention; Figure 7 It is a structural schematic diagram of the lower half ring tooling of the present invention; Figure 8 It is a side view of the core mold of the present invention; Fig. 9 It is a schematic diagram of the core mold of the present invention; Fig.10 It is a schematic diagram of the upper half ring lower mold of the present invention; Fig.11 It is a structural schematic diagram of the machining tooling of the present invention; Fig.12 It is a schematic diagram of the first manufacturing method of Comparative Example 1 of the present invention; Fig.13 It is a schematic diagram of the second manufacturing method of comparative example 1 of the present invention.
[0021] 1. Slip ring; 2. Diverter ring; 3. Upper half ring; 31. Upper half ring upper die; 32. Upper half ring lower die; 33. Core die; 34. Process groove; 35. Positioning groove; 36. Pin hole; 37. Weight reduction hole; 4. Lower half ring; 41. Upper half ring upper die; 42. Upper half ring lower die; 5. Indexing plate. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Comparative Example 1: There are two main methods for manufacturing the splitter ring: The first manufacturing method: Fig.12 As shown, it is forged into a ring shape and then machined. However, due to the thin wall thickness of the product structure, the forged ring needs to increase the packaging capacity, resulting in greater material loss; during machining, the thin wall thickness causes greater deformation, the product size is difficult to control, and the processing difficulty increases; directly using wire cutting will have a longer processing cycle.
[0024] The second manufacturing method: Fig.13 As shown in the figure, the upper and lower half rings are forged into strips and plates, then processed to product specifications, and then heated by a flame gun and bent by hammering. This method can save materials, but the forgings are thin and easy to deform, and the processing is difficult. After the material is over-fired at high temperature, its overall strength properties are reduced, the internal quality is uneven, and it does not meet the design strength requirements, which affects the service life of the product.
[0025] Embodiment 1:
[0026] like Figure 1 As shown, a method for manufacturing a shunt ring of a collector ring device, the method for manufacturing a shunt ring of a collector ring device comprises: S1: Select raw materials and perform stretching, upsetting and forging on the raw materials to obtain blanks.
[0027] The blank is made of chromium-zirconium-copper material, and the chemical composition should meet the following requirements: Zr: 0.05-0.25%, Cr: 0.50-1.50%, Cu+Cr+Zr≥99.7%, and the performance requirements should meet the following table:
[0028] After multiple process verifications and feasibility analysis after three-dimensional demonstration, the billet size, rolling specifications and feasibility of cold bending were determined.
[0029] In order to make the two groups of shunting rings used on the same equipment have the same property parameter state, a two-in-one manufacturing method is adopted. The blank is heated to 650-850℃ to make full use of its excellent plasticity. After the first fire: drawing length ≥240, upsetting height ≤120; the second fire: upsetting height ≤120, drawing, buckling. After the forging is subjected to multiple upsetting and drawing by the forging hammer, the internal metal streamline is complete and the organization is tight.
[0030] S2: Low temperature rolling is performed on the blank to obtain a plate.
[0031] In order to ensure that the blank has reliable mechanical properties, it should be rolled at low temperature. The blank is reheated to 300-350℃ and kept warm for 1-2 hours to allow the blank to be fully heated and prevent deformation from causing tearing on the surface of the material.
[0032] The billet is rolled using a rolling mill. The rolling process is carried out in multiple steps, with the deformation amount controlled at 3mm-5mm each time, and cold rolled to a predetermined size.
[0033] The forgings formed by multiple rolling have a tight internal structure, uniform metal flow lines, high performance strength, smooth surface and uniform thickness, meeting the process design requirements.
[0034] In this embodiment, the initial forging specification is φ48mm×1000mm when the blank is produced, and the rolling amount is controlled at 3mm-5mm each time. The deformation is not easy to be too large to prevent the surface forging tear marks.
[0035] S3: Cut the plate according to the size of the diverter ring and perform solution heat treatment to obtain the cut material.
[0036] The plate is cut according to the size of the diverter ring. After rolling, the forging has a high strength performance, but it cannot meet the design requirements for normal operation of the equipment. It needs to be subjected to solid solution aging heat treatment. The sheared material is aged and insulated in a furnace at 350°C to reduce the strength performance and make the internal structure more uniform, more tough, and the performance data more representative.
[0037] The heating temperature is not higher than 600℃, the temperature is evenly distributed to 350±10℃ for 1 to 3 hours, the temperature is kept for 3 hours, and the temperature is cooled to no higher than 70℃. The heat treatment process curve is as follows: Figure 5 shown.
[0038] S4: Using forming dies to cold-bend the sheared materials to obtain bent parts.
[0039] S4.1: Bend the sheared material through the upper half ring forming die.
[0040] like Figure 5 As shown, the structure of the upper half ring forming mold is mainly divided into an upper half ring upper mold, a core mold and an upper half ring lower mold.
[0041] In this embodiment, before bending, a φ19.5mm cylindrical pin is passed through the φ20mm pin hole in the upper die of the upper half ring and the core die to temporarily assemble and connect the upper die of the upper half ring and the core die. The upper and lower die process grooves are used to fix the upper and lower work surfaces of the industrial hydraulic press. The hydraulic press is lifted, and the forging is placed between the core die and the lower die and the length is evenly divided. The hydraulic press applies a downward pressure of 150-200 kN in the pressure direction, forcing the forging to bend slowly until the die is closed and then stop pressurizing; remove the φ19.5mm cylindrical pin, lift the hydraulic press to separate the upper die from the core die, take out the core die, and finally take out the bent product and reinstall the core die. Bend the next group of products.
[0042] The upper half ring is a separated 105° ring when in use. In order to ensure the accuracy and symmetry of the final product, the upper half ring needs to be formed using a one-time forming technology. In addition, the process margin will make the overall arc angle of the upper half ring greater than 210°, which will increase the difficulty of the design and production of the tooling.
[0043] In this embodiment, the upper die of the upper half ring is provided with an arc surface of R165, so that the arc segment exceeding 180° can be formed smoothly. In order to allow the sheared material to smoothly enter the upper mold cavity of the upper half ring during bending, the parting surface deviates from the center section of R165 by 15mm, and R20 arc surfaces are provided on both sides of the upper die.
[0044] In order to make the overall arc angle greater than 210° and meet the size requirements after smooth forming, a 255° arc surface is provided on the core mold and a flat surface is provided corresponding to the lower mold.
[0045] After bending, the upper die section of the upper half ring has formed an undercut of R165. At this time, the core die and the upper half ring die will be straightened again with the return traction force of the hydraulic press, causing the forming size to deviate. Therefore, the upper half ring die should be separated from the core die before demolding, and the core die should be pulled out axially after the upper half ring die returns to its position with the traction force of the hydraulic press.
[0046] The upper mold and the core mold of the upper half ring are detachable and separable structures. Figure 8 As shown, the core mold is provided with a positioning groove acting on the upper mold and a pin hole connected with the upper mold pin.
[0047] like Fig. 9 As shown, the core mold is provided with a plurality of spaced weight-reducing holes, which can effectively reduce the weight of the core mold and facilitate the removal of the core mold during the product bending process. In this embodiment, adjacent weight-reducing holes are spaced 30 degrees relative to the core mold axis.
[0048] like Fig.10 As shown, the upper die and lower die of the upper half ring are symmetrically set at 45° to match the product size, and no subsequent processing is required. The upper end of the lower die is 15mm beyond the center of the circle, so that the two ends exposed after the forging is placed in the die remain vertical, which is convenient for the upper die to run.
[0049] S4.2: Bend the sheared material through the lower half ring forming die.
[0050] like Figure 7 As shown, the structure of the lower half ring forming mold is mainly divided into a lower half ring upper mold and a lower half ring lower mold.
[0051] In this embodiment, the upper and lower die process grooves of the lower half ring are fixedly connected with the upper and lower working tables of the industrial hydraulic press. The hydraulic press is lifted, and the sheared material is placed between the upper die and the lower die and the length is evenly divided. The hydraulic press applies a downward pressure of 150-200 kN in the pressure direction, and the forging is slowly bent until the die is closed and then the pressure is stopped; the hydraulic press is lifted to separate the upper die from the lower die, and finally the bent product is taken out. The next group of products is bent.
[0052] The bending of forgings can be completed entirely within the mold cavity, making the forming convenient and quick with high dimensional accuracy.
[0053] S5: The sheared material after cold bending is machined to obtain the final forging.
[0054] After cold bending, the sheared materials need to be processed with multiple planes and holes according to the design requirements. In addition to the unfavorable factors such as the soft material, thin thickness and easy deformation of the forging, there are also requirements for the relative distribution of angles and positions during processing, which makes the entire processing process more complicated and the position tolerance difficult to control, requiring the assistance of machining tooling.
[0055] like Fig.11 As shown in the figure, the boss of the machining tool is installed concentrically with the indexing plate, and then the T-slot of the indexing plate is fastened with bolts, so that the tool and the indexing plate have strong versatility after assembly, and can be directly fixed on the workbench for product processing according to the production needs of different equipment such as boring machines, milling machines, power heads, and machining centers. During the processing process, the indexing plate is rotated by turning the hand wheel to achieve accurate distribution of the processing position.
[0056] According to the different processing positions, the position of the bolts is moved so that the bent forgings are attached and fastened to the tooling, and the planes and holes are processed in turn to the designed dimensions.
[0057] In this embodiment, the boss specification is φ60mm×5mm, and the bolts are M12 bolts.
[0058] The above process can be extended to the manufacture of similar products. The rolling range of the initial forging is 5mm-50mm, and the cold bending range is R50mm-R500mm.
[0059] The process advantages of the present invention are: Save raw materials: The forging size specification of manufacturing method 1 is: φ390mm×80mm, and the raw material consumption is 38kg / piece. The equipment uses 2 sets of products and consumes a total of 76kg of raw materials.
[0060] The forging size of manufacturing method 2 is: 1160mm×30mm×100mm. The diverter ring is processed by high-temperature bending, consuming 32kg / piece of raw materials. The equipment uses 2 sets of products and consumes a total of 64kg of raw materials.
[0061] After process optimization, the two-step forging of the diverter ring consumed a total of 16 kg of raw materials, which saved 4.75 times and 2.0 times of raw materials respectively compared with the previous two manufacturing and processing methods.
[0062] Improved mechanical properties: Mechanical data comparison:
[0063] The performance strength of the diverter ring manufactured and processed by forging ring basically meets the design requirements; the diverter ring manufactured and processed by forging plate, after high-temperature bending, samples were taken at both ends of the forging and tested, and its performance strength was greatly reduced, and there was also a significant difference in the performance strength at both ends, resulting in a great difference in the performance of the two groups of diverter ring materials used in the equipment.
[0064] The forgings formed by rolling from forged round bars have a compact internal structure, uniform metal flow lines, and high performance strength. When the forgings are subjected to solid solution aging heat treatment, they have high performance strength, so it is easy to control the performance strength within a reasonable range and make it more uniform.
[0065] 3. Time-saving processing: The two methods before optimization both require material reduction in product manufacturing. The processing equipment not only needs to select lathes, milling machines, machining centers, etc., but also needs to be segmented using saws, and the mold needs to be combined with a flame gun for hammering and bending. The process requires a lot of processing time and manpower expenditure, which is not suitable for the production needs of the workshop.
[0066] The optimized rolling process ensures that the forging thickness is 8mm, the forging surface is flat and smooth, and there are no cracks, folds, slag inclusions, etc. after visual inspection. The quality can fully meet the product design requirements. Then it is cut and divided into: 480×64×8, 680×64×8, and directly cold-bent using tooling, and finished products after stress relief.
[0067] Benefits of optimized manufacturing process: 1. No amount of forging surface needs to be removed, which shortens the processing time and can also maximize the integrity of the original metal flow lines inside the forging and the amount of heat-treated surface retention, making the product have higher strength performance and easily extending the product's service life.
[0068] 2. The cold-bending forming process is easy to master, the manufacturing process is convenient and fast, the product shape is stable and uniform, and it is suitable for mass production.
[0069] Embodiment 2:
[0070] like Figure 1 As shown, a method for manufacturing a shunt ring of a collector ring device, the method for manufacturing a shunt ring of a collector ring device comprises: S1: Select raw materials and perform stretching, upsetting and forging on the raw materials to obtain blanks.
[0071] The blank is made of chromium-zirconium-copper material, and the chemical composition should meet the following requirements: Zr: 0.05-0.25%, Cr: 0.50-1.50%, Cu+Cr+Zr≥99.7%, and the performance requirements should meet the following table:
[0072] After multiple process verifications and feasibility analysis after three-dimensional demonstration, the billet size, rolling specifications and feasibility of cold bending were determined.
[0073] In order to make the two groups of shunting rings used on the same equipment have the same property parameter state, a two-in-one manufacturing method is adopted. The blank is heated to 650-850℃ to make full use of its excellent plasticity. After the first fire: drawing length ≥240, upsetting height ≤120; the second fire: upsetting height ≤120, drawing, buckling. After the forging is subjected to multiple upsetting and drawing by the forging hammer, the internal metal streamline is complete and the organization is tight.
[0074] S2: Low temperature rolling is performed on the blank to obtain a plate.
[0075] In order to ensure that the blank has reliable mechanical properties, it should be rolled at low temperature. The blank is reheated to 300-350℃ and kept warm for 1-2 hours to allow the blank to be fully heated and prevent deformation from causing tearing on the surface of the material.
[0076] The billet is rolled using a rolling mill. The rolling process is carried out in multiple steps, with the deformation amount controlled at 3mm-5mm each time, and cold rolled to a predetermined size.
[0077] The forgings formed by multiple rolling have a tight internal structure, uniform metal flow lines, high performance strength, smooth surface and uniform thickness, meeting the process design requirements.
[0078] In this embodiment, the initial forging specification is φ48mm×1000mm when the blank is produced, and the rolling amount is controlled at 3mm-5mm each time. The deformation is not easy to be too large to prevent the surface forging tear marks.
[0079] S3: Cut the plate according to the size of the diverter ring and perform solution heat treatment to obtain the cut material.
[0080] The plate is cut according to the size of the diverter ring. After rolling, the forging has a high strength performance, but it cannot meet the design requirements for normal operation of the equipment. It needs to be subjected to solid solution aging heat treatment. The sheared material is aged and insulated in a furnace at 350°C to reduce the strength performance and make the internal structure more uniform, more tough, and the performance data more representative.
[0081] The heating temperature is not higher than 600℃, the temperature is evenly distributed to 350±10℃ for 1 to 3 hours, the temperature is kept for 3 hours, and the temperature is cooled to no higher than 70℃. The heat treatment process curve is as follows: Figure 5 shown.
[0082] S4: Conduct physical and chemical tests on the shears.
[0083] Physical and chemical tests are used to check whether the sheared materials meet the predetermined standards.
[0084] S5: Using forming dies to cold-bend the sheared materials to obtain bent parts.
[0085] S5.1: Bend the sheared material through the upper half ring forming die.
[0086] like Figure 5 As shown, the structure of the upper half ring forming mold is mainly divided into an upper half ring upper mold, a core mold and an upper half ring lower mold.
[0087] In this embodiment, before bending, a φ19.5mm cylindrical pin is passed through the φ20mm pin hole in the upper die of the upper half ring and the core die to temporarily assemble and connect the upper die of the upper half ring and the core die. The upper and lower die process grooves are used to fix the upper and lower work surfaces of the industrial hydraulic press. The hydraulic press is lifted, and the forging is placed between the core die and the lower die and the length is evenly divided. The hydraulic press applies a downward pressure of 150-200 kN in the pressure direction, forcing the forging to bend slowly until the die is closed and then stop pressurizing; remove the φ19.5mm cylindrical pin, lift the hydraulic press to separate the upper die from the core die, take out the core die, and finally take out the bent product and reinstall the core die. Bend the next group of products.
[0088] The upper half ring is a separated 105° ring when in use. In order to ensure the accuracy and symmetry of the final product, the upper half ring needs to be formed using a one-time forming technology. In addition, the process margin will make the overall arc angle of the upper half ring greater than 210°, which will increase the difficulty of the design and production of the tooling.
[0089] In this embodiment, the upper die of the upper half ring is provided with an arc surface of R165, so that the arc segment exceeding 180° can be formed smoothly. In order to allow the sheared material to smoothly enter the upper mold cavity of the upper half ring during bending, the parting surface deviates from the center section of R165 by 15mm, and R20 arc surfaces are provided on both sides of the upper die.
[0090] In order to make the overall arc angle greater than 210° and meet the size requirements after smooth forming, a 255° arc surface is provided on the core mold and a flat surface is provided corresponding to the lower mold.
[0091] After bending, the upper die section of the upper half ring has formed an undercut of R165. At this time, the core die and the upper half ring die will be straightened again with the return traction force of the hydraulic press, causing the forming size to deviate. Therefore, the upper half ring die should be separated from the core die before demolding, and the core die should be pulled out axially after the upper half ring die returns to its position with the traction force of the hydraulic press.
[0092] The upper mold and the core mold of the upper half ring are detachable and separable structures. Figure 8 As shown, the core mold is provided with a positioning groove acting on the upper mold and a pin hole connected with the upper mold pin.
[0093] like Fig. 9 As shown, the core mold is provided with a plurality of spaced weight-reducing holes, which can effectively reduce the weight of the core mold and facilitate the removal of the core mold during the product bending process. In this embodiment, adjacent weight-reducing holes are spaced 30 degrees relative to the core mold axis.
[0094] like Fig.10 As shown, the upper die and lower die of the upper half ring are symmetrically set at 45° to match the product size, and no subsequent processing is required. The upper end of the lower die is 15mm beyond the center of the circle, so that the two ends exposed after the forging is placed in the die remain vertical, which is convenient for the upper die to run.
[0095] S5.2: Bend the sheared material through the lower half ring forming die.
[0096] like Figure 7 As shown, the structural form of the lower half ring forming mold is mainly divided into a lower half ring upper mold and a lower half ring lower mold.
[0097] In this embodiment, the upper and lower die process grooves of the lower half ring are fixedly connected with the upper and lower working tables of the industrial hydraulic press. The hydraulic press is lifted, and the sheared material is placed between the upper die and the lower die and the length is evenly divided. The hydraulic press applies a downward pressure of 150-200 kN in the pressure direction, and the forging is slowly bent until the die is closed and then the pressure is stopped; the hydraulic press is lifted to separate the upper die from the lower die, and finally the bent product is taken out. The next group of products is bent.
[0098] The bending of forgings can be completed entirely within the mold cavity, making the forming convenient and quick with high dimensional accuracy.
[0099] S5: The sheared material after cold bending is machined to obtain the final forging.
[0100] After cold bending, the sheared materials need to be processed with multiple planes and holes according to the design requirements. In addition to the unfavorable factors such as the soft material, thin thickness and easy deformation of the forging, there are also requirements for the relative distribution of angles and positions during processing, which makes the entire processing process more complicated and the position tolerance difficult to control, requiring the assistance of machining tooling.
[0101] like Fig.11 As shown in the figure, the boss of the machining tool is installed concentrically with the indexing plate, and then the T-slot of the indexing plate is fastened with bolts, so that the tool and the indexing plate have strong versatility after assembly, and can be directly fixed on the workbench for product processing according to the production needs of different equipment such as boring machines, milling machines, power heads, and machining centers. During the processing process, the indexing plate is rotated by turning the hand wheel to achieve accurate distribution of the processing position.
[0102] According to the different processing positions, the position of the bolts is moved so that the bent forgings are attached and fastened to the tooling, and the planes and holes are processed in turn to the designed dimensions.
[0103] In this embodiment, the boss specification is φ60mm×5mm, and the bolts are M12 bolts.
[0104] The above process can be extended to the manufacture of similar products. The rolling range of the initial forging is 5mm-50mm, and the cold bending range is R50mm-R500mm.
[0105] The process advantages of the present invention are: Save raw materials: The forging size specification of manufacturing method 1 is: φ390mm×80mm, and the raw material consumption is 38kg / piece. The equipment uses 2 sets of products and consumes a total of 76kg of raw materials.
[0106] The forging size of manufacturing method 2 is: 1160mm×30mm×100mm. The diverter ring is processed by high-temperature bending, consuming 32kg / piece of raw materials. The equipment uses 2 sets of products and consumes a total of 64kg of raw materials.
[0107] After process optimization, the two-step forging of the diverter ring consumed a total of 16 kg of raw materials, which saved 4.75 times and 2.0 times of raw materials respectively compared with the previous two manufacturing and processing methods.
[0108] Improved mechanical properties: Mechanical data comparison:
[0109] The performance strength of the diverter ring manufactured and processed by forging ring basically meets the design requirements; the diverter ring manufactured and processed by forging plate, after high-temperature bending, samples were taken at both ends of the forging and tested, and its performance strength was greatly reduced, and there was also a significant difference in the performance strength at both ends, resulting in a great difference in the performance of the two groups of diverter ring materials used in the equipment.
[0110] The forgings formed by rolling from forged round bars have a compact internal structure, uniform metal flow lines, and high performance strength. When the forgings are subjected to solid solution aging heat treatment, they have high performance strength, so it is easy to control the performance strength within a reasonable range and make it more uniform.
[0111] 3. Time-saving processing: The two methods before optimization both require material reduction in product manufacturing. The processing equipment not only needs to select lathes, milling machines, machining centers, etc., but also needs to be segmented using saws, and the mold needs to be combined with a flame gun for hammering and bending. The process requires a lot of processing time and manpower expenditure, which is not suitable for the production needs of the workshop.
[0112] The optimized rolling process ensures that the forging thickness is 8mm, the forging surface is flat and smooth, and there are no cracks, folds, slag inclusions, etc. after visual inspection. The quality can fully meet the product design requirements. Then it is cut and divided into: 480×64×8, 680×64×8, and directly cold-bent using tooling, and finished products after stress relief.
[0113] Benefits of optimized manufacturing process: 1. No amount of forging surface needs to be removed, which shortens the processing time and can also maximize the integrity of the original metal flow lines inside the forging and the amount of heat-treated surface retention, making the product have higher strength performance and easily extending the product's service life.
[0114] 2. The cold-bending forming process is easy to master, the manufacturing process is convenient and fast, the product shape is stable and uniform, and it is suitable for mass production.
[0115] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A method for manufacturing a shunt ring of a collector ring device, It is characterized in that The manufacturing method of the shunt ring of the collector ring device comprises: Selecting raw materials and performing stretching, upsetting and forging on the raw materials to obtain blanks; The blank is subjected to low temperature rolling to obtain a plate, specifically, the blank is heated to 300-350°C, kept warm for 1-2 hours, and then rolled to obtain a plate; The plate is cut according to the size of the diverter ring and subjected to solution heat treatment to obtain the cut material; The sheared materials are cold-bent by using forming dies to obtain bent parts; The bent part is machined to obtain a diverter ring.
2. The method for manufacturing the shunt ring of the slip ring device according to claim 1, It is characterized in that The process of selecting raw materials and performing stretching and upsetting forging on the raw materials to obtain blanks is specifically to heat the selected raw materials to 650-850° C., stretch and upset the raw materials, and after the last upsetting, round the raw materials to obtain the initial forgings.
3. The method for manufacturing the shunt ring of the slip ring device according to claim 1, It is characterized in that The raw material is chromium-zirconium-copper material, wherein Zr: 0.05-0.25%, Cr: 0.50-1.50%, Cu+Cr+Zr≥99.7%.
4. The method for manufacturing the shunt ring of the slip ring device according to claim 1, It is characterized in that The blank is subjected to low temperature rolling to obtain the plate, specifically: the low temperature rolling is performed multiple times, and the deformation amount of each rolling is controlled to be 3mm~5mm.
5. The method for manufacturing the shunt ring of the slip ring device according to claim 1, It is characterized in that The forming mold comprises an upper half ring forming mold and a lower half ring forming mold. The upper half ring forming mold comprises an upper half ring upper mold, a core mold and an upper half ring lower mold. The lower half ring forming mold comprises a lower half ring upper mold and a lower half ring lower mold.
6. The method for manufacturing the shunt ring of the slip ring device according to claim 5, It is characterized in that The core mold has a 255° arc surface.
7. The method for manufacturing the shunt ring of the slip ring device according to claim 1, It is characterized in that The rolling range of the plate is 5mm-50mm, and the cold bending range of the sheared material is R50mm-R500mm.
8. A method for manufacturing a shunt ring of a slip ring device according to any one of claims 1 to 7, It is characterized in that The method of using forming dies to cold-bend the sheared materials to obtain bent parts includes: bending the sheared materials through an upper semi-ring forming die; and bending the sheared materials through a lower semi-ring forming die.
9. The method for manufacturing the shunt ring of the slip ring device according to claim 8, It is characterized in that The bending process of the sheared material by the upper half ring forming mold includes: placing the sheared material between the core mold and the upper half ring lower mold and evenly dividing the length; applying pressure along the pressure direction by a pressure device to bend the sheared material to close the mold; separating the upper half ring upper mold and the core mold to obtain a bent part.
10. The method for manufacturing the shunt ring of the slip ring device according to claim 8, It is characterized in that The sheared material is bent by a lower half-ring forming die, including: placing the sheared material between a lower half-ring upper die and a lower half-ring lower die and dividing the length evenly; applying pressure along a pressure direction by a pressure device to bend the sheared material to close the die; and separating the lower half-ring upper die and the lower half-ring lower die to obtain a bent part.
Citation Information
Patent Citations
Processing method of Cr-Zr-Cu ring
CN101602166A
Preparation method of titanium plate for deep drawing
CN107723638A
Processing method of zirconium oxygen-free copper forging rod
CN111408632A
Copper alloy material
JP2017002368A
Process for improving the bend formability of copper alloys