Preparation method of cold plate

Through the formation of a composite cold plate structure by pickling and positioning welding, the groove plates formed by the welding process is solved, and the problems of low utilization rate and long leakage detection time of welding furnaces in the manufacturing of small thin-walled cold plates are achieved, and the efficient multi-piece at one time is achieved Welding and leak detection improve manufacturing efficiency and pass rate.

CN118905583AActive Publication Date: 2024-11-08HANGZHOU SHENSHI LOW CARBON TECHNOLOGY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411167746.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The prior art is difficult to meet the efficient manufacturing needs of small and thin-walled heat exchange cold plates. The traditional diffusion welding method leads to low utilization rate of welding furnaces and a large amount of time for leakage detection.

Method used

The first and second groove plates after pickling are used for positioning welding to form the cold plate to be welded, and the stop flux is coated on both sides of the single-layer welding area to form a composite cold plate structure for diffusion welding, and then the multi-layer The layer welding area is cut and quality inspection to achieve multiple pieces of one-time welding and leakage detection.

Benefits of technology

It improves the efficiency and pass rate of diffusion welding, saves time and cost, realizes multiple pieces of one-time welding and leak detection, and improves the utilization rate and quality inspection efficiency of welding furnaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905583A_ABST
    Figure CN118905583A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a cold plate, which comprises the following steps of: coating two sides of a single-layer welding area of the cold plate to be welded with a welding stop agent, and not coating a multi-layer welding area of the cold plate to be welded with the welding stop agent; a plurality of to-be-welded cold plates are composited, laminated and rolled into a composite cold plate structure; the composite cold plate structure is put into a diffusion welding furnace to be subjected to diffusion welding, and the welded composite cold plate structure is obtained; performing product leak detection on the composite cold plate structure; and multiple layers of welding areas welded together in the qualified composite cold plate structure are cut off and split to obtain a plurality of welded cold plates. According to the method, multiple layers of cold plates can be stacked and welded, the diffusion welding efficiency of a heat exchange single sheet is improved, the single furnace utilization rate of a diffusion welding furnace is improved, and meanwhile the cost is saved; the qualified rate of diffusion welding of the heat exchange single sheet is improved, and the situation of leakage after welding is eliminated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cold plate production, and in particular to a method for preparing a cold plate. Background Art

[0002] As the heart of an aircraft, an aircraft engine is a thermomechanical device that has high requirements for precision and strength. It directly affects the overall performance of an aircraft and reflects the level of a country's scientific, industrial and national defense strength. Lightweighting is of great significance to improving the thrust-to-weight ratio, reliability, economy and safety of aircraft engines, and is one of the important research and development indicators of aircraft engines.

[0003] Titanium alloy cold plate heat exchanger has low density, high specific strength, corrosion resistance and good low-temperature toughness. At the same time, the cold plate is small in size, so it is widely used in the field of aircraft engine heat exchange.

[0004] However, with the booming development of the field of heat exchange in aviation engines, the demand for such small and thin-walled heat exchange cold plates is increasing. The traditional diffusion welding manufacturing method can no longer meet the market demand. Currently, such small and thin-walled heat exchange cold plates are mostly single-layer diffusion welded, and each piece is leak-tested after diffusion welding. This manufacturing method makes the utilization rate of the diffusion welding furnace extremely low and the leak detection consumes a lot of time. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is that currently such small and thin-walled heat exchange cold plates are mostly single-layer diffusion welded, and each piece is leak-tested individually after diffusion welding. Such manufacturing method makes the utilization rate of diffusion welding furnace extremely low and leak detection consumes a lot of time.

[0006] To this end, the present invention provides a method for preparing a cold plate, comprising:

[0007] placing the first slot plate and the second slot plate into a pickling solution for pickling;

[0008] The pickled first slot plate and the second slot plate are placed in the cold plate positioning tool, and the side of the first slot plate with the first heat dissipation slot is relatively attached to the side of the second slot plate with the second heat dissipation slot and placed in the positioning slot, and are welded and fixed to form a cold plate to be welded;

[0009] The cold plate to be welded is taken out, and a solder stop is applied on both sides of the single-layer welding area of ​​the cold plate to be welded, and no solder stop is applied on the multi-layer welding area of ​​the cold plate to be welded;

[0010] Rolling a plurality of cold plates to be welded together into a composite cold plate structure;

[0011] The composite cold plate structure is placed in a diffusion welding furnace for diffusion welding to obtain a welded composite cold plate structure;

[0012] Conduct product leak detection on composite cold plate structures;

[0013] The multi-layer welding areas welded together in the qualified composite cold plate structure are cut and split to obtain a number of welded cold plates.

[0014] Optionally, the first slot plate comprises a first slot plate body and a first welding portion, two first welding portions are provided, and the two first welding portions are provided at two ends of the same side of the first slot plate body; a first heat dissipation slot is provided on the first slot plate; and two ports of the first heat dissipation slot are respectively provided on the two first welding portions;

[0015] The second slot plate includes a second slot plate body and a second welding portion, wherein two second welding portions are provided, and the two second welding portions are provided at two ends of the same side of the second slot plate body; a second heat dissipation slot is provided on the second slot plate; and two ports of the second heat dissipation slot are respectively provided on the two second welding portions.

[0016] Optionally, the cold plate positioning tool is provided with a positioning groove for accommodating the first groove plate and the second groove plate, and is provided with a plurality of welding holes, one end of each welding hole being connected to the positioning groove;

[0017] The step of "placing the first slot plate and the second slot plate into the cold plate positioning tooling to form the cold plate to be welded" includes: an external welding device passes through the welding hole to weld and fix the first slot plate body and the second slot plate body and weld and fix the first welding part and the second welding part;

[0018] The first welding portion and the second welding portion are welded to form a multi-layer welding area; the first slot plate and the second slot plate are welded to form a single-layer welding area.

[0019] Optionally, the above step of "coating solder stop on both sides of the single-layer welding area" includes:

[0020] Paste masking tape on the side of the first welding part away from the first heat dissipation slot and the side of the second welding part away from the second heat dissipation slot; spray solder paste on both sides of the cold plate to be welded; and remove the masking tape.

[0021] Optionally, the spray thickness of the solder stopper is less than or equal to 0.01 mm.

[0022] Optionally, the above step of “diffusion welding the composite cold plate structure” includes:

[0023] Place the composite cold plate structure into the diffusion welding furnace, close the furnace door, and evacuate to 10 -2Pa and above; heating the composite cold plate structure and keeping it warm; pressurizing and welding the composite cold plate structure body after it reaches the preset temperature; and maintaining the pressure for the preset time.

[0024] Optionally, the above step of "heating and keeping the composite cold plate structure warm" includes: heating to 350°C in a diffusion welding furnace and keeping warm for 60 minutes; heating to 700°C in a diffusion welding furnace and keeping warm for 90 minutes; heating to 900°C in a diffusion welding furnace and keeping warm for 100 minutes.

[0025] Optionally, the above step of “pressurizing and welding the composite cold plate structure body after it reaches a preset temperature” includes:

[0026] When the monitored temperature of the composite cold plate structure reaches 900°C, the timing starts for pressurization, the pressure is set at 3-5MPa, and the pressure is maintained for 60 minutes.

[0027] Optionally, the cold plate is further provided with two detection holes, the detection holes penetrate the cold plate, and the two detection holes are respectively connected to two ends of a heat dissipation channel enclosed by the first heat dissipation slot and the second heat dissipation slot;

[0028] The step of "performing product leak detection on the composite cold plate structure" includes: welding a needle valve on the top surface of the composite cold plate structure completed by diffusion welding, the bottom end of the needle valve is connected to the detection hole, one side of the needle valve is connected to the airtight testing equipment, and the other side is connected to the pressure gauge to inflate the detection hole; ensuring that the heat dissipation channel in the composite cold plate structure completed by diffusion welding is in an airtight environment of 3MPa for pressure maintenance; if the product has no deformation and no leakage, it is marked as qualified, and if the product has leakage or deformation, it is marked as unqualified.

[0029] Optionally, the pickling solution mentioned above includes hydrofluoric acid, nitric acid and water, and the ratio of hydrofluoric acid: nitric acid: water = 0.96: 4.74: 94.3.

[0030] The technical solution provided by the present invention has the following advantages:

[0031] 1. The preparation method of the cold plate provided by the present invention comprises: placing a first slot plate and a second slot plate into a pickling solution for pickling; placing the pickled first slot plate and the second slot plate into a cold plate positioning tool, placing a side surface of the first slot plate with a first heat dissipation slot and a side surface of the second slot plate with a second heat dissipation slot relatively in contact with each other and placing them in the positioning slot, and welding and fixing them to form a cold plate to be welded; taking out the cold plate to be welded, applying a solder stopper on both sides of the single-layer welding area of ​​the cold plate to be welded, and not applying a solder stopper on the multi-layer welding area of ​​the cold plate to be welded; rolling a plurality of cold plates to be welded into a composite cold plate structure; placing the composite cold plate structure into a diffusion welding furnace for diffusion welding to obtain a welded composite cold plate structure; performing product leak detection on the composite cold plate structure; cutting and splitting the multi-layer welding areas welded together in a qualified composite cold plate structure to obtain a plurality of welded cold plates.

[0032] This method can stack and weld multiple layers of cold plates. By using the above method, multiple pieces can be welded in one furnace and multiple pieces can be leak tested at one time, thus saving a lot of time and cost. At the same time, the qualified rate of diffusion welding is also guaranteed.

[0033] 2. The first and second slot plates are pickled with a pickling solution. This is to remove the dense oxide film on the surface and expose the silvery white metallic luster of the product. The pickling solution includes hydrofluoric acid, nitric acid and water, and the ratio of hydrofluoric acid: nitric acid: water = 0.96: 4.74: 94.3. The pickling time is one minute. Since diffusion welding requires that there is no oxide layer on the surface of the parts, the presence of the oxide layer will hinder the diffusion of atoms during the diffusion welding process. At the same time, this ratio concentration and pickling time can just remove the oxide layer of the parts without corroding the part matrix; laying the foundation for obtaining high-quality diffusion welding joints.

[0034] 3. After the welding provided by the present invention is completed, the multi-piece welding areas of the thirty layers are welded together; therefore, the detection holes opened on the multi-layer welding areas are welded and fixed to form two vertical detection channels. Two needle valves are welded on the top surface of the composite cold plate structure after diffusion welding, and the two needle valves are fixed corresponding to the two detection holes. The bottom ends of the two needle valves are connected to the detection holes, so that the two needle valves are connected to the detection channels. One side of the needle valve is connected to the airtight test equipment, and the other side is connected to the pressure gauge; one of the needle valves is used as the air inlet end, and the other needle valve is kept sealed, and one of the detection channels is slowly inflated through the airtight test equipment; the gas can be inflated into the heat dissipation channel in the thirty-layer cold plate at the same time, ensuring that the heat dissipation channel in the composite cold plate structure after diffusion welding is in an airtight environment of 3MPa, and the pressure is maintained for 15 minutes; if the product has no deformation and no leakage, it is marked as qualified, and if the product has leakage or deformation, it is marked as unqualified. Masking paper is used for protection, multi-layer welding and single-layer welding are partitioned, and leak detection can be performed on the multi-layer cold plate at the same time, which improves the quality inspection efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 A flow chart of a method for preparing a cold plate provided by the present invention;

[0037] Figure 2 A schematic diagram of the structure of a cold plate to be welded in the method for preparing a cold plate provided by the present invention;

[0038] Figure 3 A schematic diagram of the structure of a cold plate positioning tool in the cold plate preparation method provided by the present invention;

[0039] Figure 4 A schematic diagram of the structure in which a cold plate to be welded is installed in a cold plate positioning tool in the cold plate preparation method provided by the present invention;

[0040] Figure 5 A schematic diagram of the structure of attaching masking paper to the multi-layer welding area of ​​the cold plate to be welded in the method for preparing the cold plate provided by the present invention;

[0041] Figure 6 A schematic diagram of the structure of spraying solder stop on a cold plate to be welded with masking paper in the preparation method of the cold plate provided by the present invention;

[0042] Figure 7 A schematic diagram of the structure of the composite cold plate provided by the present invention;

[0043] Figure 8 A schematic diagram of a structure in which the composite cold plate structure provided by the present invention is placed between an upper pressure head and a lower pressure head;

[0044] Fig. 9 A schematic diagram of the structure between the upper pressure head and the lower pressure head for placing multiple composite cold plates provided by the present invention;

[0045] Fig.10 A schematic diagram of the structure of a conventional diffusion welding device with an uneven upper pressure head provided by the present invention;

[0046] Fig.11 A schematic diagram of a diffusion welding temperature rise curve provided by the present invention;

[0047] Fig.12 Provides a schematic diagram of the installation of a needle valve and a composite cold plate structure for the present invention;

[0048] Description of reference numerals:

[0049] 1-cold plate to be welded; 11-single-layer welding area; 12-multi-layer welding area; 13-detection hole;

[0050] 2-cold plate positioning tool; 21-positioning groove; 22-welding hole;

[0051] 31 - upper pressure head; 32 - lower pressure head; 33 - welding tool;

[0052] 4-composite cold plate structure; 41-hole-free side plate;

[0053] 5-Needle valve. DETAILED DESCRIPTION

[0054] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0055] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0056] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0057] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0058] Example

[0059] This embodiment provides a method for preparing a cold plate, such as Figures 1 to 12As shown, the following are required: a cold plate positioning tool 2 and a pressurizing device. The shape of the cold plate positioning tool 2 is consistent with the shape of the cold plate 1 to be welded. Taking this embodiment as an example, the cold plate 1 to be welded is U-shaped, and the cold plate positioning tool 2 is also U-shaped. The outer dimensions of the cold plate positioning tool 2 are larger than the outer dimensions of the cold plate positioning tool 2. A positioning groove 21 is provided on one side of the cold plate positioning tool 2. The shape and size of the positioning groove 21 are the same as those of the cold plate positioning tool 2. A plurality of welding holes 22 are provided at the edge of the positioning groove 21. One end of the welding hole 22 is connected to the positioning groove 21, and the other end is connected to the outside. In the present application, Figure 3 As shown, welding holes 22 are respectively provided on both sides of the upper end, the two side edges and the bottom end of the positioning groove 21 .

[0060] like Figure 8 As shown, the pressurizing device includes an upper press head 31 and a lower press head 32, and the opposing surfaces of the upper press head 31 and the lower press head 32 are both horizontal planes. The cold plate 1 to be welded is placed between the upper press head 31 and the lower press head 32 for welding. If necessary, a welding tool 33 made of graphite can be placed between the upper press head 31 and the lower press head 32.

[0061] The cold plate 1 to be welded is assembled from a first slot plate and a second slot plate. In this embodiment, both the first slot plate and the second slot plate are U-shaped. Two first welding parts are fixed at the two ends of the same side of the first slot plate body. A first heat dissipation slot is provided on one side of the first slot plate. Two ports of the first heat dissipation slot are respectively arranged on the two first welding parts, and the middle part of the first heat dissipation slot is provided on the first slot plate body; two second welding parts are fixed at the two ends of the same side of the second slot plate body. A second heat dissipation slot is provided on one side of the second slot plate. Two ports of the second heat dissipation slot are respectively arranged on the two first welding parts, and the middle part of the second heat dissipation slot is provided on the second slot plate body. The shapes of the first heat dissipation slot and the second heat dissipation slot are matched. The side of the first slot plate with the first heat dissipation slot and the side of the second slot plate with the second heat dissipation slot are relatively attached together, and the first welding part and the second welding part are also attached together to form the cold plate 1 to be welded.

[0062] Furthermore, the two first welding parts are each provided with a first through hole, the two second welding parts are each provided with a second through hole, and the two first through holes and the two second through holes are arranged in a one-to-one correspondence to form two detection holes 13 .

[0063] It should be noted that the cold plate, the cold plate positioning tool 2 and the positioning groove 21 can be in any shape and are not limited to the above-mentioned U-shape. The three must be arranged accordingly.

[0064] like Figure 1 As shown, the preparation method of the cold plate provided in this embodiment specifically includes the following steps:

[0065] S1. Pickle the first and second slot plates with a pickling solution. To remove the dense oxide film on the surface, so that the product reveals a silvery white metallic luster. The pickling solution includes hydrofluoric acid, nitric acid and water, hydrofluoric acid: nitric acid: water = 0.96: 4.74: 94.3. The pickling time is one minute. Since diffusion welding requires that there is no oxide layer on the surface of the parts, the presence of the oxide layer will hinder the diffusion of atoms during the diffusion welding process. At the same time, this ratio concentration and pickling time can just remove the oxide layer of the parts without corroding the part matrix; laying the foundation for obtaining high-quality diffusion welding joints.

[0066] S2, assemble the cold plate 1 to be welded. Figures 2 to 4 As shown, the first slot plate is placed into the positioning slot 21 with the side facing away from the first heat dissipation slot toward the bottom of the positioning slot 21, and then the side of the second slot plate with the second heat dissipation slot facing the first slot plate is placed into the positioning slot 21. At this time, the first heat dissipation slot and the second heat dissipation slot are correspondingly fitted together, and the first heat dissipation slot and the second heat dissipation slot can cooperate with each other to form a heat dissipation pipe to achieve the heat dissipation function. The first welding part and the second welding part are also fitted together. Through the welding hole 22, the first slot plate and the second slot plate are spot welded with high precision, and the first welding part and the second welding part are spot welded with high precision, so as to position the shape of the first slot plate and the second slot plate. The first welding part and the second welding part are welded to form a multi-layer welding area 12; the first slot plate and the second slot plate are welded to form a single-layer welding area 11.

[0067] The first slot plate and the first welding part form the upper slot plate, the second slot body and the second welding part form the lower slot plate, the single-side gap between the positioning slot 21 and the upper slot plate and the lower slot plate shall not be greater than 0.02mm, and the upper slot plate and the lower slot plate shall not be misaligned by performing micro-arc cold spot welding positioning on the product shape. The docking accuracy of the heat dissipation channel between the first slot plate and the second slot plate is ensured, effectively reducing the defect rate.

[0068] S3, apply solder stop on both sides of the single-layer welding area 11. Figure 5 and Figure 6 As shown, masking tape is pasted on the side of the first welding part away from the first heat dissipation slot and the side of the second welding part away from the second heat dissipation slot. Generally speaking, the width of the first welding part and the second welding part is 8mm, and double-sided pasting ensures that the pasting is firm and there must be no missing parts.

[0069] Then, use a spray gun to spray solder stop on the surface of the single-layer welding area 11, i.e., the first slot plate and the second slot plate. The solder stop spray thickness shall not be greater than 0.01 mm. After spraying, remove the masking tape to ensure that the masking tape pasted area, i.e., the multi-layer welding area 12, is not exposed to the solder stop.

[0070] S4, rolling a plurality of cold plates into a composite cold plate structure 4. Figure 7 As shown, the titanium alloy heat exchange cold plate that has been spot welded is fixed by stacking and fixing by shape positioning to form a composite cold plate structure 4. The number of stacking layers is thirty and shall not be greater than thirty. Two layers of non-porous side plates 41 are placed at the bottom of the thirty-layer composite cold plate structure 4. The surface of the non-porous side plates 41 also needs to be sprayed with anti-soldering agent before stacking.

[0071] S5, diffusion welding the composite cold plate structure 4. Figures 8 to 11 As shown, the composite cold plate structure 4 is placed in a diffusion welding furnace, the furnace door is closed, and the vacuum is pumped to 10 -2 Pa and above, the temperature is raised to 350°C in 30 minutes, and kept warm for 60 minutes; then the temperature in the diffusion welding furnace is raised to 700°C in 30 minutes, and kept warm for 90 minutes; the diffusion welding furnace is raised to 900°C in 10 minutes, and kept warm for 100 minutes. When the monitored temperature reaches 900°C, the timing is started and the pressurization is set at a rate of 0.05mm / min, and the pressure is set to 3-5MPa. After keeping the pressure for 60 minutes, the equipment can be cooled down; a welded cold plate composite structure is obtained, because the multi-layer welding area 12, that is, the first welding part and the second welding part, is not sprayed with solder stopper, and the single-piece welding area, that is, the first slot plate body and the second slot plate body, is sprayed with solder stopper, so after the welding is completed, the multi-piece welding areas of the thirty layers are welded together; and the single-piece welding area is only the first slot plate body and the second slot plate body on a single cold plate are welded together, and the adjacent cold plates are not welded and fixed.

[0072] In this embodiment, by observing the displacement of the equipment, it is ensured that the total displacement of the cold plate is 1.5 mm.

[0073] 900℃ and 3-5MPa are the best temperature and pressure for diffusion welding of this material. At the same time, the temperature is raised in multiple stages to ensure that the product can be fully heated through to avoid the core temperature being too low to affect diffusion welding; the slow pressing speed of 0.05mm / min and the deformation of 1.5mm are conducive to the diffusion of atoms in the diffusion welding process of the parts. The product can finally form reliable diffusion welding through the above optimal process parameters.

[0074] S6, perform product leak detection on the composite cold plate structure 4 after diffusion welding. As can be seen from step S5, after welding, the multi-layer welding areas of the thirty layers are welded together; therefore, the detection holes 13 opened on the multi-layer welding area 12 are welded and fixed to form two vertical detection channels. Fig.12As shown, two needle valves 5 are welded on the top surface of the composite cold plate structure 4 after diffusion welding, and the two needle valves 5 are fixed corresponding to the two detection holes 13. The bottom ends of the two needle valves 5 are connected to the detection holes 13, so that the two needle valves 5 are connected to the detection channels, one side of the needle valve 5 is connected to the airtight testing equipment, and the other side is connected to the pressure gauge; one of the needle valves 5 is used as the air inlet end, and the other needle valve 5 remains sealed, and one of the detection channels is slowly inflated through the airtight testing equipment; the gas can be inflated into the heat dissipation channels in the thirty-layer cold plate at the same time, ensuring that the heat dissipation channels in the composite cold plate structure 4 after diffusion welding are in an airtight environment of 3MPa, and the pressure is maintained for 15 minutes; if the product has no deformation and no leakage, it is marked as qualified, and if the product has leakage or deformation, it is marked as unqualified.

[0075] By using the above method, multiple pieces can be welded in one furnace and multiple pieces can be leak-checked at one time, thus saving a lot of time and cost. At the same time, the qualified rate of diffusion welding is also guaranteed. Specifically, the air tightness test of thirty layers of cold plates can be carried out at the same time, which greatly improves the production efficiency; by using the above method, this method can stack and weld thirty layers of cold plates, improve the diffusion welding efficiency of the heat exchange single piece, improve the utilization rate of the single furnace of the diffusion welding furnace, and save costs at the same time; improve the qualified rate of the diffusion welding of the heat exchange single piece, and eliminate the leakage after welding. Through the protection of masking paper, multi-layer welding and single-layer welding are partitioned, and leak detection can be carried out on multiple layers of cold plates at the same time, which improves the quality inspection efficiency.

[0076] In other practicable embodiments, the composite cold plate structure 4 can be placed between the upper pressure head 31 and the lower pressure head 32, using Fig. 9 As shown, five of them can be arranged between the upper pressure head 31 and the lower pressure head 32. A welding fixture 33 can also be placed between the upper pressure head 31 and the lower pressure head 32, and five composite cold plate structures 4 can be placed above and below the welding fixture 33, respectively, to improve production efficiency. When installing the welding fixture 33, since the thickness of a single cold plate is 1.6mm, the single piece diffusion welding deformation is required to be 0.05mm. At this time, the parallelism and flatness requirements of the equipment pressure head and the welding fixture 33 (upper pressure head 31 and lower pressure head 32) and the graphite plate (welding fixture 33) are extremely strict to avoid the product from appearing Fig.10 If the weld is not completed, the airtight test will result in leakage.

[0077] When thirty layers of cold plates are stacked for welding at the same time, the deformation of a single piece is still 0.05mm, and the total deformation is 1.5mm. At this time, the influence of the tilt and unevenness of the equipment pressure head can be eliminated, ensuring that all welding surfaces are ultimately subjected to stress.

[0078] In other feasible embodiments, before the composite cold plate structure 4 is placed in the diffusion welding furnace, a non-porous side plate is also fixed at the top of the composite cold plate structure, and a through hole is also opened on the non-porous side plate above the composite cold plate structure 4 corresponding to the detection hole, and the through hole is connected to the detection hole. The through hole and the detection hole together form a detection channel, and solder stopper is applied on the non-porous side plate. When a needle valve is needed to detect leaks, the needle valve needs to be installed in the through hole on the non-porous side plate corresponding to the needle valve. The detection channel is used to detect thirty layers of cold plates at the same time, thereby avoiding the situation where the top cold plate is scrapped during routine inspections, thereby reducing production costs.

[0079] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a cold plate, characterized in that: include: placing the first slot plate and the second slot plate into a pickling solution for pickling; Placing the pickled first slot plate and the second slot plate into a cold plate positioning tool (2), placing a side surface of the first slot plate with a first heat dissipation slot and a side surface of the second slot plate with a second heat dissipation slot opposite to each other and placing them in a positioning slot (21), and welding and fixing them to form a cold plate (1) to be welded; The cold plate (1) to be welded is taken out, and a solder stopper is applied to both sides of the single-layer welding area (11) of the cold plate (1) to be welded, and a solder stopper is not applied to the multi-layer welding area (12) of the cold plate (1) to be welded; Compound-stacked and rolled a plurality of cold plates to be welded (1) into a compound cold plate structure (4); Placing the composite cold plate structure (4) into a diffusion welding furnace for diffusion welding to obtain a welded composite cold plate structure (4); Conducting product leak detection on the composite cold plate structure (4); The multi-layer welding area (12) welded together in the qualified composite cold plate structure (4) is cut and split to obtain a plurality of welded cold plates.

2. The method for preparing a cold plate according to claim 1, characterized in that: The first slot plate comprises a first slot plate body and a first welding portion, wherein two first welding portions are provided, and the two first welding portions are provided at two ends of the same side of the first slot plate body; a first heat dissipation slot is provided on the first slot plate; and two ports of the first heat dissipation slot are respectively provided on the two first welding portions; The second slot plate includes a second slot plate body and a second welding portion, wherein two second welding portions are provided, and the two second welding portions are provided at two ends of the same side of the second slot plate body; a second heat dissipation slot is provided on the second slot plate; and two ports of the second heat dissipation slot are respectively provided on the two second welding portions.

3. The method for preparing a cold plate according to claim 2, characterized in that: The cold plate positioning tool (2) is provided with a positioning groove (21) for accommodating the first groove plate and the second groove plate, and is provided with a plurality of welding holes (22), one end of the welding hole (22) being connected to the positioning groove (21); The step of "placing the first slot plate and the second slot plate in the cold plate positioning tool (2) and fixing them to form the cold plate to be welded (1)" comprises: an external welding device passes through the welding hole (22) to weld and fix the first slot plate body and the second slot plate body and to weld and fix the first welding portion and the second welding portion; The first welding portion and the second welding portion are welded to form a multi-layer welding area (12); the first slot plate and the second slot plate are welded to form a single-layer welding area (11).

4. The method for preparing a cold plate according to claim 3, characterized in that: The step of "coating solder stop on both sides of the single-layer soldering area (11)" includes: Masking tape is pasted on the side of the first welding portion facing away from the first heat dissipation slot and the side of the second welding portion facing away from the second heat dissipation slot; solder stopper is sprayed on both sides of the cold plate (1) to be welded; and the masking tape is removed.

5. The method for preparing a cold plate according to claim 4, characterized in that: The spraying thickness of the solder stopper is less than or equal to 0.01 mm.

6. The method for preparing a cold plate according to claim 5, characterized in that: The step of "diffusion welding the composite cold plate structure (4)" comprises: Place the composite cold plate structure (4) into the diffusion welding furnace, close the furnace door, and evacuate to 10 -2 Pa and above; heating the composite cold plate structure (4) and keeping it warm; pressurizing and welding the composite cold plate structure (4) after the body reaches a preset temperature; and maintaining the pressure for a preset time.

7. The method for preparing a cold plate according to claim 6, characterized in that: The step of "heating and keeping the composite cold plate structure (4) warm" includes: heating to 350°C in a diffusion welding furnace and keeping warm for 60 minutes; heating to 700°C in a diffusion welding furnace and keeping warm for 90 minutes; heating to 900°C in a diffusion welding furnace and keeping warm for 100 minutes.

8. The method for preparing a cold plate according to claim 6, characterized in that: The step of "pressurizing and welding the composite cold plate structure (4) after the body reaches a preset temperature" includes: When the monitored temperature of the composite cold plate structure (4) reaches 900°C, the timing starts and the pressurization is started. The pressure is set to 3-5MPa and the pressure is maintained for 60 minutes.

9. The method for preparing a cold plate according to claim 6, characterized in that: The cold plate is also provided with two detection holes (13), the detection holes (13) passing through the cold plate, and the two detection holes (13) are respectively connected to two ends of a heat dissipation channel enclosed by the first heat dissipation slot and the second heat dissipation slot; The step of "performing a product leak test on the composite cold plate structure (4)" comprises: welding a needle valve (5) on the top surface of the composite cold plate structure (4) after diffusion welding, the bottom end of the needle valve (5) being connected to the detection hole (13), one side of the needle valve (5) being connected to an airtight testing device, and the other side being connected to a pressure gauge, and inflating air into the detection hole (13); ensuring that the heat dissipation channel in the composite cold plate structure (4) after diffusion welding is in an airtight environment of 3MPa for pressure maintenance; if the product has no deformation and no leakage, it is marked as qualified, and if the product has leakage or deformation, it is marked as unqualified.

10. The method for preparing a cold plate according to any one of claims 1 to 8, characterized in that: The pickling solution includes hydrofluoric acid, nitric acid and water, and the ratio of hydrofluoric acid: nitric acid: water is 0.96: 4.74: 94.3.

Citation Information

Patent Citations

  • Pack rolling production method of titanium steel composite board

    CN103817149A

  • Heat exchanger processing method and heat exchanger

    CN106808173A

  • Plate bundle processing method for plate-fin heat exchanger

    CN109813158A

  • Manufacturing method of micro-channel cold plates

    CN109848666A

  • Double-sided laminated airtight brazing system and method in 3D microwave radio frequency module

    CN112453617A