Protection, temperature adjustment and sensing integrated intelligent protection layer structure and preparation method and application thereof
By designing an integrated intelligent protection layer for temperature regulation and perception on the submarine, combining PVDF sensors, phase change microcapsules and conductive nanoparticles, the dual threat of submarine under extreme cold and explosion shock waves is solved, and more efficient temperature regulation is achieved. Damage assessment improves the submarine's endurance and internal environmental stability.
Patent Information
- Application Number
- CN202410952442.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
Submarines face the dual threat of extreme cold temperature and explosion shock waves in harsh underwater environments. The existing technology lacks effective temperature regulation and explosion perception capabilities, making it difficult to improve the protection performance and adaptability of submarines.
A integrated intelligent protective layer of protection, temperature regulation and perception is designed, including sensor array layer, inner and outer phase change protection layer and explosion-proof protection layer. The submarine is improved by using PVDF sensors, phase change microcapsules and conductive nanoparticles. explosion-proof performance and temperature regulation capability.
It improves the explosion-proof performance and temperature adaptability of the submarine, can promptly detect and evaluate damage, improves the endurance and internal environmental stability of the submarine, and saves energy for cooling and heating.
Smart Images

Figure CN118906511A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of armor protection technology, and in particular to a protective temperature regulation and sensing integrated intelligent protective layer structure, and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] The harsh underwater temperature environment in the submarine mission area will threaten the life safety of the crew. For example, the ice layer in the Arctic Ocean can play a concealing role and prevent submarines from being detected in the water, but the extremely cold temperature in the Arctic severely limits the submarine's lurking time. On the other hand, the submarine hull will be subject to a variety of security threats underwater, mainly explosion shock waves. In order to protect the submarine hull and crew, excellent explosion-proof materials and technology for timely detection of hull damage are particularly critical. They can not only reduce the damage to the hull, but also promptly detect the location of the hull damage and assess the degree of damage, which is conducive to quickly formulating emergency repair plans and improving the vitality of the submarine.
[0004] Phase change materials, as a material that can store and release heat energy, can control the internal environment temperature. Currently, phase change materials are made into phase change microcapsules in the fields of building energy conservation, textiles, thermal energy, etc., and have achieved good results. However, there are few studies on their application as a temperature regulating protective layer on the surface of submarines. On the other hand, the self-sensing technology of submarines is mainly concentrated in sonar systems, underwater communications, etc., and the perception technology of explosion shock waves is still relatively lacking.
[0005] Therefore, developing an integrated protective layer that can be applied to the surface of submarines and has high explosion resistance, explosion sensing, and energy storage and temperature regulation capabilities has become one of the urgent issues to be solved. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a protective temperature regulation and sensing integrated intelligent protective layer structure and its preparation method and application, which can improve the submarine's ability to resist shock waves while realizing timely discovery and assessment of its own damage, so as to improve the submarine's ability to adapt to harsh temperature environments.
[0007] In order to achieve the above object, the technical solution of the present invention is:
[0008] In the first aspect, a protective temperature regulating and sensing integrated intelligent protective layer structure, the protective layers are distributed on both the inner and outer sides of the submarine hull: the outer side of the submarine hull includes a sensor array layer, an inner phase change protective layer, an outer phase change protective layer and an explosion-proof protective layer distributed from the inside to the outside; the inner side of the submarine hull includes an inner hull phase change protective layer;
[0009] The sensor array layer includes a plurality of PVDF sensors arranged in an array, and the PVDF sensor includes: a PVDF-HFP film covered on an aluminum plate, and conductive nanoparticles are dispersed in the PVDF-HFP film;
[0010] The explosion-proof protective layer is obtained by combining a plurality of sheet-shaped explosion-proof protective layer materials. The raw materials for preparing the explosion-proof protective layer materials include: isocyanate and amino compound in a molar ratio of (0.9-1.3):1, and nano-enhanced particles are dispersed in the explosion-proof protective layer materials;
[0011] The inner phase change protective layer, the outer phase change protective layer and the phase change protective layer inside the shell are respectively obtained by combining a plurality of flaky phase change protective layer materials, and the structure of the phase change protective layer material is: phase change microcapsules with a particle size of 1 to 1000 μm are uniformly dispersed inside the explosion-proof protective layer material; the raw materials for preparing the phase change microcapsule wall include: isocyanate and amino compound with a molar ratio of (1.05 to 1.2):1, and the phase change material is filled in the cavity of the phase change microcapsule;
[0012] The phase change material includes one or more of butyl stearate, paraffin, n-octadecane and polyethylene glycol.
[0013] In a second aspect, the method for preparing the above-mentioned protective temperature regulating and sensing integrated intelligent protective layer comprises the following steps:
[0014] S1, weighing PVDF-HFP powder and DMF solvent in a mass ratio of 1: (2.5-3), adding nano conductive powder, stirring evenly and degassing to obtain a first mixed solution;
[0015] S2, injecting the first mixed solution into a mold at 80-100°C, heat-curing to obtain a film, stretching the film to a thickness of 0.3-1.2 mm, pasting an aluminum foil electrode on the stretched film, standing to cure, and then fixing the stretched film and the aluminum foil electrode on an aluminum plate with a thickness of 4-20 mm to obtain a PVDF sensor;
[0016] S3, adding nano-reinforced particles to the amino compound to disperse evenly, heating to remove bubbles and mixing with isocyanate, heating in a water bath in a vacuum environment for a set time to obtain a second mixed solution;
[0017] S4, drying the second mixed liquid under a vacuum environment to obtain a solid sheet-like explosion-proof protective layer material;
[0018] S5, taking a set amount of isocyanate and phase change material and stirring to form an oil phase, taking a set amount of deionized water and an emulsifier and stirring to form a water phase, and under heating and stirring conditions, according to a water-to-oil mass ratio of (6-10):1, slowly adding the oil phase to the water phase, and continuously stirring to form an oil-in-water emulsion;
[0019] S6, taking a set amount of amino compound and mixing it with deionized water to form an amino compound solution, dropping the amino compound solution into the stirred oil-in-water emulsion, continuously stirring and heating the reaction to obtain a third mixed solution, filtering the third mixed solution, washing it with distilled water and anhydrous ethanol respectively, and then drying it to obtain powdery phase change microcapsules, uniformly adding the obtained phase change microcapsules to the second mixed solution obtained in S3, and then drying it under a vacuum environment to obtain a solid sheet-like phase change protective layer material;
[0020] S7. Fix PVDF sensors on the outer surface of the shell in an array arrangement to form a sensor array layer, fix phase change protective layer materials on the outside of the sensor array layer to form an inner phase change protective layer, fix phase change protective layer materials on the outside of the inner phase change protective layer to form an outer phase change protective layer, fix explosion-proof protective layer materials on the outside of the outer phase change protective layer material to form an explosion-proof protective layer, and fix phase change protective layer materials on the inner surface of the shell to form an inner phase change protective layer of the shell.
[0021] Optionally, in S7, the fixing method is: mechanically fixing the connection with bolts, or fixing with epoxy resin.
[0022] In a third aspect, the present invention provides the application of the above-mentioned protective temperature regulation and sensing integrated intelligent protective layer in submarine protection.
[0023] The beneficial effects of the present invention are:
[0024] 1. The present invention provides an intelligent protective layer integrating protection, temperature regulation and perception, which further improves the explosion-proof performance of submarines by adding a protective layer; and makes up for the shortcomings of modern submarines' perception technology when working underwater, and can detect their own explosions and damage, which is conducive to timely assessing the location and extent of damage, quickly formulating emergency repair plans, and improving the vitality of submarines; two phase change materials on the outer surface plus one phase change material on the inner surface can not only freely select phase change materials according to the working environment temperature to adapt to different environments, but also increase the stability of the internal environment temperature of the submarine. The use of the protective layer of the present invention can not only greatly improve the submarine's ability to adapt to the ambient temperature, but also save energy used for cooling and heating the internal environment.
[0025] 2. The present invention proposes a new research idea for the field of submarine protection, improves the adaptability of submarines to harsh environments, and further improves the endurance of submarines. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0027] Figure 1 This is a schematic diagram of the protective layer structure of a submarine hull having a composite protective temperature regulating and sensing integrated intelligent protective layer prepared in Example 1; wherein: 1. submarine hull; 2. sensor array layer; 3. high-temperature phase change protective layer; 4. low-temperature phase change protective layer; 5. explosion-proof protective layer; 6. room-temperature phase change protective layer.
[0028] Figure 2 Schematic diagram of the preparation process of the explosion-proof protective layer material in Example 1.
[0029] Figure 3 Schematic diagram of the preparation process of the phase change protective layer material in Example 1.
[0030] Figure 4 Schematic diagram of the preparation process of the PVDF sensor of Example 1.
[0031] Figure 5 Graph showing the relationship between the thickness of the explosion-proof protective layer and the peak pressure in Example 1.
[0032] Figure 6 This is the DSC curve of the room temperature phase change protective layer in Example 1. DETAILED DESCRIPTION
[0033] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0034] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in the text are for demonstration purposes only.
[0035] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0036] The present invention provides an intelligent protective layer structure with integrated protection, temperature regulation and perception, wherein the protective layers are distributed on both the inner and outer sides of a submarine hull: the outer side of the submarine hull includes a sensor array layer, an inner phase change protective layer, an outer phase change protective layer and an explosion-proof protective layer which are distributed from the inside to the outside; the inner side of the submarine hull includes an inner hull phase change protective layer;
[0037] The sensor array layer includes a plurality of PVDF sensors arranged in an array, and the PVDF sensor includes: a PVDF-HFP film covered on an aluminum plate, and conductive nanoparticles are dispersed in the PVDF-HFP film;
[0038] The explosion-proof protective layer is obtained by combining a plurality of sheet-shaped explosion-proof protective layer materials. The raw materials for preparing the explosion-proof protective layer materials include: isocyanate and amino compound in a molar ratio of (0.9-1.3):1, and nano-enhanced particles are dispersed in the explosion-proof protective layer materials;
[0039] The inner phase change protective layer, the outer phase change protective layer and the phase change protective layer inside the shell are respectively obtained by combining a plurality of flaky phase change protective layer materials. The structure of the phase change protective layer material is as follows: phase change microcapsules with a particle size of 1 to 1000 μm are uniformly dispersed inside the explosion-proof protective layer material; the raw materials for preparing the phase change microcapsule wall include: isocyanate and amino compound with a molar ratio of (1.05 to 1.2):1, and the phase change material is filled in the cavity of the phase change microcapsule;
[0040] The phase change material includes one or more of butyl stearate, paraffin, n-octadecane and polyethylene glycol.
[0041] The sensor array layer is composed of polyvinylidene fluoride (PVDF) sensors, which have nanosecond response time and high stress sensitivity, and can provide new sensing methods beyond sonar systems and underwater communications.
[0042] Polyurea is a new type of polymer material formed by the polymerization of isocyanate components and terminal amino substances. Its molecular chain is composed of soft segments and hard segments connected alternately. In recent years, domestic and foreign scholars have made many efforts in the research on the shock wave attenuation mechanism and law of polyurea elastomers. Polyurea has high wear resistance, corrosion resistance, and flexibility, and can fully buffer and absorb the energy of explosion shock waves. In the present invention, polyurea materials are used to prepare explosion-proof protective layers and phase change protective layers, which improves the bonding ability between different protective layers and is conducive to further improving the overall performance of the protective layer.
[0043] Optionally, the conductive nanoparticles include: one or more of carbon nanotubes (MWNT) and vapor grown carbon nanofibers (VGCF), and the mass ratio of the conductive nanoparticles to PVDF-HFP is (0.0005-0.003):1.
[0044] Optionally, the isocyanate includes one or more of carbodiimide-modified diphenylmethane diisocyanate (carbodiimide-modified MDI), diphenylmethane diisocyanate (MDI) and toluene diisocyanate (TDI).
[0045] Optionally, the amino compound includes one or more of poly-1,4-butylene glycol bis(4-aminobenzoate), diethylenetriamine and triethylenetetramine.
[0046] Optionally, the nano-reinforced particles include: one or more of silicon dioxide, carbon nanotubes, graphene and hollow glass microspheres, the diameter of the nano-reinforced particles is 10-50 nm, and the mass proportion of the nano-reinforced particles in the explosion-proof protective layer is 1-2%.
[0047] Optionally, the inner phase-change protective layer includes a high-temperature phase-change protective layer, the outer phase-change protective layer includes a low-temperature phase-change protective layer; and the inner phase-change protective layer of the shell includes a room-temperature phase-change protective layer;
[0048] Alternatively, the inner phase-change protective layer includes a low-temperature phase-change protective layer, the outer phase-change protective layer includes a high-temperature phase-change protective layer; and the inner phase-change protective layer of the shell includes a room-temperature phase-change protective layer;
[0049] The phase change temperature of the phase change material in the low-temperature phase change protective layer is 0-10°C higher than the low-temperature working environment temperature, preferably 5-20°C; the phase change temperature of the phase change material in the high-temperature phase change protective layer is 0-10°C lower than the high-temperature working environment temperature, preferably 28-40°C.
[0050] Optionally, the phase change temperature of the phase change material in the room temperature phase change protection layer is 16-26°C.
[0051] Optionally, the sensor array layer includes a PVDF sensor and a wire connected to the PVDF sensor, and the wire passes through the protective temperature regulation and sensing integrated intelligent protection layer and is connected to a signal acquisition processor.
[0052] Optionally, the thickness of the sensor array layer is 0.5-2 cm, and the gaps between the wires are filled with insulating resin.
[0053] Optionally, the explosion-proof protective layer has a thickness of 0.3 to 3 cm.
[0054] Optionally, the thickness of the inner phase change protective layer is 0.5 to 3 cm, preferably, the thickness is 1 to 2 cm.
[0055] Optionally, the thickness of the outer phase change protective layer is 0.5 to 3 cm, preferably, the thickness is 1 to 2 cm.
[0056] The present invention provides a method for preparing the above-mentioned protective temperature regulation and sensing integrated intelligent protective layer, comprising the following steps:
[0057] S1, weighing PVDF-HFP powder and DMF solvent in a mass ratio of 1: (2.5-3), adding nano conductive powder, stirring evenly and degassing to obtain a first mixed solution;
[0058] S2, injecting the first mixed solution into a mold at 80-100°C, heat-curing to obtain a film, stretching the film to a thickness of 0.3-1.2 mm, pasting an aluminum foil electrode on the stretched film, standing to cure, and then fixing the stretched film and the aluminum foil electrode on an aluminum plate with a thickness of 4-20 mm to obtain a PVDF sensor;
[0059] S3, adding nano-reinforced particles to the amino compound to disperse evenly, heating to remove bubbles and mixing with isocyanate, heating in a water bath in a vacuum environment for a set time to obtain a second mixed solution;
[0060] S4, drying the second mixed liquid under a vacuum environment to obtain a solid sheet-like explosion-proof protective layer material;
[0061] S5, taking a set amount of isocyanate and phase change material and stirring to form an oil phase, taking a set amount of deionized water and an emulsifier and stirring to form a water phase, and under heating and stirring conditions, according to a water-to-oil mass ratio of (6-10):1, slowly adding the oil phase to the water phase, and continuously stirring to form an oil-in-water emulsion;
[0062] S6, taking a set amount of amino compound and mixing it with deionized water to form an amino compound solution, dropping the amino compound solution into the stirred oil-in-water emulsion, continuously stirring and heating the reaction to obtain a third mixed solution, filtering the third mixed solution, washing it with distilled water and anhydrous ethanol respectively, and then drying it to obtain powdery phase change microcapsules, uniformly adding the obtained phase change microcapsules to the second mixed solution obtained in S3, and then drying it under a vacuum environment to obtain a solid sheet-like phase change protective layer material;
[0063] S7. Fix PVDF sensors on the outer surface of the shell in an array arrangement to form a sensor array layer, fix phase change protective layer materials on the outside of the sensor array layer to form an inner phase change protective layer, fix phase change protective layer materials on the outside of the inner phase change protective layer to form an outer phase change protective layer, fix explosion-proof protective layer materials on the outside of the outer phase change protective layer material to form an explosion-proof protective layer, fix phase change protective layer materials on the outside of the explosion-proof protective layer to form an outer phase change protective layer, and fix phase change protective layer materials on the inner surface of the shell to form an inner phase change protective layer of the shell.
[0064] Optionally, in S1, a set amount of nanoparticles is weighed and added to an N,N-dimethylformamide (DMF) solution, and ultrasonic stirring is performed for 15 minutes to obtain a suspension, a set amount of PVDF-HFP powder is added to the suspension and stirred at a speed of 1500-2500 r / min for 10 minutes to obtain a mixed solution, and the mixed solution is stirred under ultrasonic waves for 5 minutes, and then the mixed solution is placed in a stirrer and stirred at a speed of 1500-2500 r / min for 10 minutes, and degassed for 1 minute.
[0065] Optionally, in S2, an aluminum plate of suitable size is used as a back plate and heated and maintained at 90°C, and the back plate is surrounded by four outer aluminum plates of suitable size, and the mixed liquid obtained in step 1 is poured in until the enclosed space is filled. After 5 to 10 minutes, the four aluminum plates are removed, and the temperature is kept constant. After 2 to 3 hours, the cured film is removed; then the cured film is placed on a universal testing machine for stretching, and the middle square uniform part of the stretched film is taken as a film sample, and an aluminum foil electrode is glued to the film sample using conductive glue, and it is left to stand for 24 hours. After curing using the distributed electrode method, it is fixed to the aluminum plate using epoxy resin.
[0066] Specifically, the thickness of the aluminum plate back plate is 1-2 mm, preferably 1 mm; the thickness of the outer aluminum plate is 2-3 mm, preferably 2.5 mm.
[0067] Optionally, in S2, the stretching ratio is 300-500% by area; the stretching rate is 5-20 mm / min, preferably, 10 mm / min.
[0068] Optionally, in S2, the stretching temperature is 55-65°C.
[0069] Optionally, in S2, the side length of the film sample before stretching is 3 to 5 cm.
[0070] Optionally, in S2, the distributed electrode method polarization time is 8 minutes, the pause time is 4 minutes, and the polarization electric field is 8 to 60 MV / m.
[0071] Optionally, in S3, nano-reinforced particles are added to the amino compound, and an ultrasonic water bath dispersion method is used to disperse the nano-reinforced particles in the amino compound for a set time to form a uniform mixed solution; then the mixed solution is placed in a vacuum oven to remove bubbles, and is taken out after drying for a certain period of time.
[0072] Specifically, water bath heating is performed in a vacuum environment in a reaction kettle with a polytetrafluoroethylene protective layer.
[0073] Optionally, in S3, the water bath temperature is 55-65° C., the ultrasonic dispersion frequency is 60-80 Hz, and the dispersion time is 10-15 min.
[0074] Optionally, in S3, the oven temperature is 60-70° C., and the drying time is 0.5-2 h.
[0075] Optionally, in S4, the vacuum drying temperature is 60-75° C., and the drying time is 50-70 min, preferably 60 min.
[0076] Specifically, the two mixed liquids are introduced into a mold with a polytetrafluoroethylene protective layer, and then the mold is placed in a vacuum oven for drying.
[0077] Optionally, in S5, the emulsifier includes: one or more of alkylphenol polyoxyethylene ether (OP-10), polystyrene maleic anhydride (SMA), and polyoxyethylene sorbitan monooleate (TW-80).
[0078] Optionally, in S5, the emulsifier accounts for 2 to 4 wt % of the oil phase.
[0079] Optionally, in S5, the heating and stirring conditions are: the heating temperature is 25-35° C., and the speed of the magnetic stirrer is 4000-10000 r / min.
[0080] Optionally, in S5, the stirring is continued for 5 to 10 minutes.
[0081] Optionally, in S6, the mass ratio of the amino compound to deionized water is: 1:(3-5).
[0082] Optionally, in S6, the dripping method is: dripping using a peristaltic pump, and the dripping speed is: 1 to 3 mL / min.
[0083] Optionally, in S6, the stirring speed of the water-in-oil emulsion is 200-300 r / min, and the heating temperature of the heating reaction is 55-65°C.
[0084] Optionally, in S6, washing is performed twice with distilled water and twice with anhydrous ethanol respectively.
[0085] Optionally, in S6, the drying temperature is 65-80° C., and the drying time is 12-24 hours.
[0086] Optionally, in S7, at least one PVDF sensor is arranged per square decimeter outside the shell.
[0087] The present invention provides an application of the above-mentioned protective temperature regulation and sensing integrated intelligent protective layer in submarine protection, specifically: the above-mentioned protective temperature regulation and sensing integrated intelligent protective layer is arranged on the outside of the shell, and the room temperature phase change material is fixed on the inner surface of the shell.
[0088] Example 1
[0089] like Figure 2As shown, silica particles with a diameter of 20 nm are added to 70g of poly-1,4-butylene glycol bis(4-aminobenzoate), and an ultrasonic water bath dispersion method is used with a dispersion frequency of 70Hz and maintained at a heating temperature of 60°C for 15min, so that the silica is dispersed in the poly-1,4-butylene glycol bis(4-aminobenzoate) to form a uniform mixed solution. The obtained mixed solution is placed in a vacuum oven at 70°C for 1h to remove bubbles. The solution after excluding bubbles and 30g of carbodiimide-modified MDI are added to a reactor with a polytetrafluoroethylene protective layer, stirred for 5min in a vacuum environment and a water bath temperature of 60°C to obtain a second mixed solution, and then the second mixed solution is poured into a polytetrafluoroethylene mold, and continuously dried for 1h in an environment of 70°C to obtain a solid sheet-like explosion-proof protective layer material; the explosion-proof protective layer material obtained in this embodiment is solidified into explosion-proof protective materials of different thicknesses, and a shock wave tube is used to load a shock wave pressure test system to apply a shock wave to the explosion-proof protective material for testing, and a non-explosion-proof protective layer ( Figure 5 The peak pressure of the wall surface corresponds to the destruction of the explosion-proof protective layer of different thicknesses (when the thickness is 0) and the set peak pressure of the wall surface; the peak pressure of the wall surface refers to the pressure value of the first peak after the wall surface pressure surges after the shock wave pressure is loaded. The lower the value, the better the explosion-proof effect; Figure 5 As shown, when the thickness reaches 15 mm, the drop in peak pressure tends to be gentle, reaching below 175 kPa. Therefore, in this embodiment, a solid sheet-like explosion-proof protective layer material with a thickness of 15 mm is assembled as the protective layer of the submarine hull.
[0090] like Figure 4As shown, 0.02 g of carbon nanotubes were weighed and added to 30 g of N,N-dimethylformamide solution, and dispersed by ultrasonic stirring for 15 min to obtain a suspension, 10 g of PVDF-HFP powder was added to the suspension and stirred at a speed of 2000 r / min for 10 min to obtain a mixed solution, and then the mixed solution was stirred and dispersed under ultrasonic waves for 5 min, and then the mixed solution was placed in a stirrer and stirred at a speed of 2000 r / min for 10 min, and then degassed for 1 min to obtain a first mixed solution, and an aluminum plate with a size of 20 cm × 10 cm × 1 mm was heated to 90 ° C as a back plate and kept warm, and four outer aluminum plates with a thickness of 2.5 mm and a width of 3 cm were used to form the back plate. Surround it, pour the obtained mixed liquid into it until the enclosed space is filled. After 7 minutes, remove the four outer aluminum plates and keep the temperature at 90℃. After 2h, take down the film cured by PVDF-HFP material; place the cured film on a universal testing machine and stretch it at 60℃ with a stretching ratio of 500%; the stretching rate is 10mm / min, take a 3cm×3cm uniform part in the center of the stretched film as a film sample (thickness is 0.6±0.05mm), use conductive glue to stick aluminum foil electrodes on the film sample, let it stand for 24h, then use the distributed electrode method to cure it, and then use epoxy resin to fix it on an aluminum plate with a thickness of 12mm to form a PVDF sensor.
[0091] like Figure 3 As shown, 3g of carbodiimide modified MDI and 10g of butyl stearate (the selected phase change material) are mixed in a container and stirred manually to form an oil phase, and 90g of distilled water and 0.26g of emulsifier OP-10 are stirred and mixed in another container to form an aqueous phase; the aqueous phase is placed in a magnetic stirrer, the speed is set to 4000r / min, and the temperature is maintained at 35°C for 5min; then the oil phase is slowly added to the aqueous phase and stirred for 5min to form an oil-in-water emulsion; 7g of poly-1,4-butylene glycol bis(4-aminobenzoate) is weighed and mixed with 25g of distilled water, and the solution is pumped into the solution at a speed of 300r / min by a peristaltic pump. Add to the emulsion at a dropwise addition rate of 1 mL / min; after the dropwise addition is completed, maintain a rotation speed of 300 r / min, raise the temperature to 60°C, react for a period of time to obtain a third mixed solution, filter the third mixed solution, wash it twice with distilled water and anhydrous ethanol, put it in an 80°C drying oven and dry it for 12 hours to obtain powdered phase change microcapsules, then add the phase change microcapsules to the second mixed solution prepared in this embodiment, pour the second mixed solution with the phase change microcapsules into a polytetrafluoroethylene mold, and continue drying it in an environment of 70°C for 1 hour to obtain a solid sheet-like room temperature phase change protective layer material; after testing, the DSC curve of the room temperature phase change protective layer material obtained in this embodiment is as shown in FIG. Figure 6As shown, its phase change temperature is 17.19°C and the phase change latent heat is 97.61J / g. It can absorb latent heat and play a role in maintaining the stability of the internal environment temperature.
[0092] In addition, the phase change materials selected are: paraffin with a phase change temperature of 5°C and paraffin with a phase change temperature of 30°C, and the low-temperature phase change protective layer material and the high-temperature phase change protective layer material are respectively made according to the above steps.
[0093] The prepared phase change protective layer materials are all solid sheet materials with a thickness of 10 mm.
[0094] The PVDF sensors are evenly distributed on the outer surface of the submarine hull with a density of at least 1 per square decimeter to form a PVDF sensor array, and the gaps in this layer are filled with insulating epoxy resin. A 1cm thick solid sheet high-temperature phase change protective layer material is fixed on the outside with bolts or epoxy resin is pasted to solidify. A 1cm thick low-temperature phase change protective layer material is fixed on the outside of the high-temperature phase change protective layer with bolts or epoxy resin is pasted. A 1.5cm explosion-proof protective layer material is fixed on the outside of the low-temperature phase change protective layer with bolts or epoxy resin is pasted. Then, a 1cm thick room-temperature phase change protective layer material is fixed on the inner surface of the submarine hull with bolts or epoxy resin is pasted. The submarine hull obtained is as follows. Figure 1 As shown, the outer structure of the submarine hull 1 includes a sensor array layer 2, a high-temperature phase change protective layer 3, a low-temperature phase change protective layer 4 and an explosion-proof protective layer 5 which are distributed in sequence from the inside to the outside; the inner structure of the submarine hull 1 includes a room-temperature phase change protective layer; the explosion-proof protective layer 5 and the PVDF sensor array in the sensor array layer 2 can respectively achieve effective protection and perception of shock waves, and the low-temperature phase change protective layer 4 and the high-temperature phase change protective layer 5 can respectively adapt to the external extremely cold and hot environments; the room-temperature phase change protective layer 6 is used to maintain the temperature inside the submarine.
[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An intelligent protective layer structure with integrated protection, temperature regulation and perception, It is characterized in that The protective layers are distributed on both the inner and outer sides of the submarine hull: the outer side of the submarine hull includes a sensor array layer, an inner phase change protective layer, an outer phase change protective layer and an explosion-proof protective layer which are distributed from the inside to the outside; the inner side of the submarine hull includes an inner phase change protective layer; The sensor array layer includes a plurality of PVDF sensors arranged in an array, and the PVDF sensor includes: a PVDF-HFP film covered on an aluminum plate, and conductive nanoparticles are dispersed in the PVDF-HFP film; The explosion-proof protective layer is obtained by combining a plurality of sheet-shaped explosion-proof protective layer materials, wherein the preparation raw materials of the explosion-proof protective layer materials include: isocyanate and amino compound in a molar ratio of (0.9-1.3):1, and nano-enhanced particles are dispersed in the explosion-proof protective layer materials; The inner phase-change protective layer, the outer phase-change protective layer and the phase-change protective layer inside the shell are respectively obtained by combining a plurality of flaky phase-change protective layer materials, and the structure of the phase-change protective layer material is as follows: phase-change microcapsules with a particle size of 1 to 1000 μm are uniformly dispersed inside the explosion-proof protective layer material; the raw materials for preparing the wall of the phase-change microcapsule include: isocyanate and amino compound with a molar ratio of (1.05 to 1.2):1, and the phase-change material is filled in the cavity of the phase-change microcapsule; The phase change material includes one or more of butyl stearate, paraffin, n-octadecane and polyethylene glycol.
2. According to the protection temperature regulation perception integrated intelligent protective layer structure of claim 1, It is characterized in that The conductive nanoparticles include: one or more of carbon nanotubes and vapor-grown carbon nanofibers, and the mass ratio of the conductive nanoparticles to PVDF-HFP is (0.0005-0.003):
1.
3. The intelligent protective layer structure with integrated protection, temperature regulation and perception according to claim 1, It is characterized in that The nano-enhanced particles include one or more of silicon dioxide, carbon nanotubes, graphene and hollow glass microspheres. The diameter of the nano-enhanced particles is 10-50 nm, and the mass proportion of the nano-enhanced particles in the explosion-proof protective layer is 1-2%.
4. The protection temperature regulation and perception integrated intelligent protective layer structure according to claim 1, It is characterized in that Isocyanates include: One or more of carbodiimide-modified diphenylmethane diisocyanate, diphenylmethane diisocyanate and toluene diisocyanate; Optionally, the amino compound includes one or more of poly-1,4-butylene glycol bis(4-aminobenzoate), diethylenetriamine and triethylenetetramine.
5. According to the protection temperature regulation perception integrated intelligent protective layer structure of claim 1, It is characterized in that The inner phase change protection layer includes a high temperature phase change protection layer, the outer phase change protection layer includes a low temperature phase change protection layer; the inner phase change protection layer of the shell includes a room temperature phase change protection layer; The inner phase change protection layer includes a low-temperature phase change protection layer, the outer phase change protection layer includes a high-temperature phase change protection layer; the inner phase change protection layer of the shell includes a room-temperature phase change protection layer; The phase change temperature of the phase change material in the low-temperature phase change protective layer is 0 to 10°C higher than the low-temperature working environment temperature, preferably 5 to 20°C; the phase change temperature of the phase change material in the high-temperature phase change protective layer is 0 to 10°C lower than the high-temperature working environment temperature, preferably 28 to 40°C; Optionally, the phase change temperature of the phase change material in the room temperature phase change protection layer is 16-26°C.
6. A method for preparing a protective temperature regulating and sensing integrated intelligent protective layer structure according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1, weighing PVDF-HFP powder and DMF solvent in a mass ratio of 1: (2.5-3), adding nano conductive powder, stirring evenly and degassing to obtain a first mixed solution; S2, injecting the first mixed solution into a mold at 80-100°C, heat-curing to obtain a film, stretching the film to a thickness of 0.3-1.2 mm, pasting an aluminum foil electrode on the stretched film, standing to cure, and then fixing the stretched film and the aluminum foil electrode on an aluminum plate with a thickness of 4-20 mm to obtain a PVDF sensor; S3, adding nano-reinforced particles to the amino compound to disperse evenly, heating to remove bubbles and mixing with isocyanate, heating in a water bath in a vacuum environment for a set time to obtain a second mixed solution; S4, drying the second mixed liquid under vacuum to obtain a solid sheet-like explosion-proof protective layer material; S5, taking a set amount of isocyanate and phase change material and stirring to form an oil phase, taking a set amount of deionized water and an emulsifier and stirring to form a water phase, and under heating and stirring conditions, according to a water-to-oil mass ratio of (6-10):1, slowly adding the oil phase to the water phase, and continuously stirring to form an oil-in-water emulsion; S6, taking a set amount of amino compound and mixing it with deionized water to form an amino compound solution, dropping the amino compound solution into the stirred oil-in-water emulsion, continuously stirring and heating the reaction to obtain a third mixed solution, filtering the third mixed solution, washing it with distilled water and anhydrous ethanol respectively, and then drying it to obtain powdery phase change microcapsules, uniformly adding the obtained phase change microcapsules to the second mixed solution obtained in S3, and then drying it under a vacuum environment to obtain a solid sheet-like phase change protective layer material; S7. Fix PVDF sensors on the outer surface of the shell in an array arrangement to form a sensor array layer, fix phase change protective layer materials on the outside of the sensor array layer to form an inner phase change protective layer, fix phase change protective layer materials on the outside of the inner phase change protective layer to form an outer phase change protective layer, fix explosion-proof protective layer materials on the outside of the outer phase change protective layer material to form an explosion-proof protective layer, fix phase change protective layer materials on the outside of the explosion-proof protective layer to form an outer phase change protective layer, and fix phase change protective layer materials on the inner surface of the shell to form an inner phase change protective layer of the shell.
7. The method for preparing the protective temperature regulating and sensing integrated intelligent protective layer structure according to claim 6, It is characterized in that In S1, a set amount of nanoparticles is weighed and added to an N,N-dimethylformamide solution, and ultrasonic stirring is performed for 15 minutes to obtain a suspension. A set amount of PVDF-HFP powder is added to the suspension and stirred at a speed of 1500 to 2500 r / min for 10 minutes to obtain a mixed solution, and the mixed solution is stirred under ultrasonic waves for 5 minutes. The mixed solution is then placed in a stirrer and stirred at a speed of 1500 to 2500 r / min for 10 minutes, and degassed for 1 minute.
8. The method for preparing the protective temperature regulation and sensing integrated intelligent protective layer structure according to claim 6, It is characterized in that In S2, a piece of aluminum plate of suitable size is used as a back plate and heated to maintain 90°C, and four aluminum plates of suitable size are used to surround the bottom plate, and the mixed solution obtained in step 1 is poured in until the enclosed space is filled. After 5 to 10 minutes, the four aluminum plates are removed, and the temperature is kept constant. After 2 to 3 hours, the cured film is removed; then the cured film is placed on a universal testing machine for stretching, and the middle square uniform part of the stretched film is taken as a film sample. Aluminum foil electrodes are glued to the film sample using conductive glue, and the film sample is left to stand for 24 hours. After being cured using the distributed electrode method, it is fixed on the aluminum plate using epoxy resin; Optionally, in S2, the stretching ratio is area ratio: 300-500%; the stretching rate is 5-20 mm / min, preferably 10 mm / min; Optionally, in S2, the stretching temperature is 55 to 65°C; Optionally, in S2, the side length of the film sample before stretching is: 3 to 5 cm; Optionally, in S2, the distributed electrode method polarization time is 8 minutes, the pause time is 4 minutes, and the polarization electric field is 8 to 60 MV / m.
9. The method for preparing the protective temperature regulation and sensing integrated intelligent protective layer structure according to claim 6, It is characterized in that In S3, nano-enhanced particles are added to the amino compound, and an ultrasonic water bath dispersion method is used to disperse the nano-enhanced particles in the amino compound for a set time to form a uniform mixed solution; then the mixed solution is placed in a vacuum oven to remove bubbles, and is taken out after drying for a certain period of time; Optionally, in S3, the water bath temperature is 55-65° C., the ultrasonic dispersion frequency is 60-80 Hz, and the dispersion time is 10-15 min; Optionally, in S3, the oven temperature is 60-70° C., and the drying time is 0.5-2 h; In S4, the vacuum drying temperature is 60-75°C, and the drying time is 50-70 min, preferably 60 min; Optionally, in S5, the emulsifier includes: one or more of alkylphenol polyoxyethylene ether, polystyrene maleic anhydride, and polyoxyethylene sorbitan monooleate; Optionally, in S5, the emulsifier accounts for 2 to 4 wt % of the oil phase; Optionally, in S5, the heating and stirring conditions are: the heating temperature is 25 to 35° C., and the speed of the magnetic stirrer is 4000 to 10000 r / min; Optionally, in S5, the stirring time is continued for 5 to 10 minutes; Optionally, in S6, the mass ratio of the amino compound to deionized water is 1:(3-5); Optionally, in S6, the dripping method is: dripping using a peristaltic pump, and the dripping speed is: 1 to 3 mL / min; Optionally, in S6, the stirring speed of the oil-in-water emulsion is 200-300 r / min, and the heating temperature of the heating reaction is 55-65° C.; Optionally, in S6, washing with distilled water and anhydrous ethanol twice respectively; Optionally, in S6, the drying temperature is 65 to 80° C., and the drying time is 12 to 24 hours; Optionally, in S7, at least one PVDF sensor is arranged per square decimeter outside the shell; Optionally, in S7, a room temperature phase change material is fixed on the inner surface of the shell.
10. An application of the protective temperature regulation and sensing integrated intelligent protective layer structure as described in any one of claims 1 to 5 in submarine protection.