Preparation method and application of oxygen-doped porous helical carbon nanotube
Doping oxygen atoms on the spiral carbon nanotubes by thermal oxidation method to form oxygen-doped porous materials, solving the complex and high cost problem of preparing heteroatom-doped porous carbon materials in the prior art, and achieving low-cost and easy-to-preparation Oxygen doped porous helical carbon nanotubes increase specific surface area and are suitable for electromagnetic wave absorption and supercapacitors.
Patent Information
- Application Number
- CN202410994863.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, when preparing porous carbon-based materials with heteroatom doping, the method is complex and costly, making it difficult to achieve a simple and easy preparation process.
Thermal oxidation method is used to create pores on three-dimensional spiral carbon nanotubes and dopant oxygen atoms to form porous materials with three-dimensional spiral chiral structures. Through one-step thermal strategy processing technology, amorphous polycrystalline coexistence is used to use spiral carbon nanotubes with amorphous polycrystalline coexistence. As a raw material, the thermal oxidation temperature and time are controlled to form oxygen-doped porous helical carbon nanotubes coexisting with micro-meta-macropores.
It realizes low-cost, easy-to-regulate oxygen-doped porous spiral carbon nanotube preparation, significantly improves the specific surface area, is suitable for electromagnetic wave absorption and supercapacitors, and provides broad application prospects.
Smart Images

Figure CN118908188A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of novel material preparation, and in particular to a preparation method and application of oxygen-doped porous helical carbon nanotubes. Background Art
[0002] The special advantages of defects and heteroatom doping in carbon networks in terms of electromagnetic properties provide inspiration for the design of advanced carbon-based microwave absorbing materials. In addition, defects and heteroatoms can provide efficient and available storage sites for the adsorption of ions during electrochemical energy storage, and increase the specific surface area to promote the formation of double-layer capacitance, making electrochemical energy storage mainly surface-controlled, thereby ensuring the reversible performance and rate performance of carbon materials as electrochemical energy storage materials. Therefore, it is very necessary to find a method for preparing porous carbon-based materials with heteroatom doping.
[0003] At present, freezing, carbonization and activation of carbon-rich precursors are the main methods for preparing porous carbon-based materials with heteroatom doping and porous structure. For example, an instantaneous freezing-assisted template strategy for preparing three-dimensional hierarchical porous carbon nanosheets embedded with CoFe2O4 particles has been reported, in which the optimized composite absorber exhibits a minimum reflection loss value of -52.29 dB at a low filling ratio of 20wt% [Chemical Engineering Journal 427 (2022) 130796]. Another study used ice template method, followed by carbonization treatment, to obtain nitrogen-doped porous carbon aerogels, which showed an effective absorption bandwidth of 7.36GHz at a low filling ratio of 10wt% [Nano-Micro Lett. (2024) 16: 16]. On the other hand, triethylamine (TEA) can be used as an acid acceptor to condense polycyclotriphosphine-4,40-sulfonyldiphenol (PZS) at room temperature, and then porous carbon spheres can be obtained after carbonization and removal of the SiOx template. The porous carbon spheres have a good hierarchical porous structure (micropores, mesopores and macropores), providing more ion transport channels and fast reaction kinetics. They have excellent rate performance and long cycle stability when used as electrodes [J. Mater. Chem. A 12 (10) 6489-6498 (2022)]; a colloidal solution of polyvinyl pyrrolidone (PVP), urea and zinc nitrate can be pre-foamed, carbonized and the zinc oxide template removed to obtain a porous nanosheet foam structure (NPCNs). The NPCNs cathode has sufficient physical and chemical zinc storage sites in the mesopores and micropores and around the nitrogen doping, and the NPCNs have fast electron / ion pathways in the two-dimensional direction [Small 16 (18) 2108057 (2022)]. As a three-dimensional carbon skeleton material, helical carbon nanotubes have advantages in many fields (thermoelectrics, electrochemistry, sensing and microwave absorption) due to their high thermal conductivity, stable physicochemical properties and the superelastic network they form.
[0004] However, due to the high cost and complex process of the above method, it is not easy to prepare, so there is an urgent need for a simple preparation method of heteroatom-doped hierarchical porous carbon material. To this end, we propose a preparation method and application of oxygen-doped porous helical carbon nanotubes. Summary of the invention
[0005] The present invention mainly solves the technical problems existing in the above-mentioned prior art and provides a preparation method and application of oxygen-doped porous helical carbon nanotubes.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a porous spiral carbon nanotube with oxygen doping, with three-dimensional spiral carbon nanotube as the skeleton, and pores are formed on the three-dimensional spiral carbon nanotube by thermal oxidation method while oxygen atoms are doped to form a porous material with a three-dimensional spiral chiral structure.
[0007] As a further limitation of the above scheme, the three-dimensional helical carbon nanotube is synthesized by chemical vapor deposition and has both sp 2 and sp 3 Hybrid amorphous-polycrystalline structure.
[0008] A method for preparing oxygen-doped porous spiral carbon nanotubes, using spiral carbon nanotubes or spiral carbon nanotubes subjected to high-temperature carbonization as raw materials, preferentially removing the amorphous carbon part in the spiral carbon nanotubes by thermal oxidation, while the amorphous carbon part is oxidized and removed, forming a pore structure, and the carbon atoms around the pores are reconstructed and combined with oxygen atoms to form oxygen-containing functional groups.
[0009] As a preferred technical solution of the present invention, the following preparation steps are specifically included:
[0010] S1: using spiral carbon nanotubes or spiral carbon nanotubes treated by high temperature carbonization as raw materials;
[0011] S2: Place the raw material of S1 in a chamber of a thermal oxidation heating device with an oxygen or air atmosphere, raise the temperature to 400-600°C at 1-20°C / min, start the constant temperature program, and keep it for 0-1h to obtain a series of micro-meso-macroporous samples;
[0012] S3: Cool the series of micro-mesoporous and macroporous samples prepared in S2 to room temperature and then take them out.
[0013] As a further limitation of the above scheme, the high-temperature carbonization treatment method of the spiral carbon nanotube raw material in S1 is to place the spiral carbon nanotube in an inert gas atmosphere such as nitrogen or argon, and heat it to above 700°C for carbonization treatment. The commonly used carbonization temperature is between 900°C and 1200°C.
[0014] As a further limitation of the above scheme, in S2, the spiral carbon nanotubes or the spiral carbon nanotubes after high-temperature carbonization are placed in an oxygen-containing atmosphere such as air or oxygen, heated to between 500°C and 600°C for thermal oxidation to form pores, and at the same time, oxygen atoms are doped into the carbon network around the pores.
[0015] As a preferred technical solution of the present invention, the thermal oxidation heating device includes any one of a combustion heating device, a resistance heating device, an induction heating device, a microwave heating device and a radiation heating device.
[0016] An application of oxygen-doped porous helical carbon nanotubes, wherein the porous helical carbon nanotubes are applied to electromagnetic wave absorption and supercapacitors.
[0017] Beneficial Effects
[0018] The invention provides a preparation method of oxygen-doped porous spiral carbon nanotubes and applications thereof.
[0019] It has the following beneficial effects:
[0020] 1. The present invention uses amorphous and polycrystalline coexisting helical carbon nanotubes as raw materials, and obtains oxygen-doped porous helical carbon nanotubes through only one step of thermal strategy treatment technology. The pore-making process is simple and easy, and the experimental conditions are relatively low. In addition, the thermal strategy technology has the advantages of low cost and easy regulation.
[0021] 2. In the preparation process of the present invention, by controlling the thermal oxidation temperature and time, part of the amorphous carbon of the spiral carbon nanotube is oxidized and then etched into micropores or mesopores, and at the same time, part of the oxygen atoms are incorporated into the surrounding carbon network.
[0022] 3. The oxygen-doped porous spiral carbon nanotubes prepared by the present invention have periodic macropores and exhibit the coexistence of micro (~0.8nm) and mesopores (~0.4nm). By adjusting the thermal oxidation temperature and time, compared with the original carbon nanotubes, the oxygen-doped porous carbon nanotubes prepared by the present invention retain the long-range conductive network while greatly improving the specific surface area.
[0023] 4. Oxygen-doped porous helical carbon nanotubes are used as absorbers. The absorption frequency band can cover the C, X and Ku bands of the radar band, and the widest effective absorption bandwidth can reach 7.3GHz. In addition, this structure is also conducive to the formation of double-layer capacitance at the electrolyte-electrode interface. At the same time, a large amount of oxygen doping and carbon defects provide efficient ion storage sites, which can greatly improve the specific capacity of the capacitor. Therefore, this material has broad application prospects in the field of electromagnetic wave absorption and supercapacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the conditions under which the present invention can be implemented, so they have no substantial technical significance.
[0025] Figure 1 is a SEM image of the helical carbon nanotube prepared in Example 2;
[0026] Figure 2 is a SEM image of the oxygen-doped porous helical carbon nanotube prepared in Example 3;
[0027] Figure 3 is a SEM image of the oxygen-doped porous helical carbon nanotube prepared in Example 4;
[0028] Figure 4 is a SEM image of the helical carbon nanotube prepared in Example 5;
[0029] Figure 5 The nitrogen adsorption-desorption curve and pore size distribution diagram of the helical carbon nanotubes prepared in Example 2;
[0030] Figure 6 The nitrogen adsorption-desorption curve and pore size distribution diagram of the oxygen-doped porous helical carbon nanotube prepared in Example 3;
[0031] Figure 7 The nitrogen adsorption-desorption curve and pore size distribution diagram of the oxygen-doped porous helical carbon nanotube prepared in Example 4;
[0032] Figure 8 The nitrogen adsorption-desorption curve and pore size distribution diagram of the oxygen-doped porous helical carbon nanotube prepared in Example 5;
[0033] Fig. 9 The cyclic voltammetry (CV) diagram of the self-supporting and oxygen-doped porous helical carbon nanotube film electrodes prepared in Example 3;
[0034] Fig.10 This is a graph of reflection loss (absorption performance) of the oxygen-doped porous helical carbon nanotube-based microwave absorber prepared in Example 4;
[0035] Fig.11 This is a graph of the reflection loss (wave absorption performance) of the oxygen-doped porous helical carbon nanotube-based microwave absorber prepared in Example 5. DETAILED DESCRIPTION
[0036] Example 1
[0037] See also Figure 1-10 A porous spiral carbon nanotube doped with oxygen has a three-dimensional spiral carbon nanotube as the skeleton. The three-dimensional spiral carbon nanotube is pore-formed by thermal oxidation and oxygen atoms are doped at the same time to form a porous material with a three-dimensional spiral chiral structure.
[0038] Three-dimensional helical carbon nanotubes are synthesized by chemical vapor deposition and have a hybrid amorphous-polycrystalline structure.
[0039] A method for preparing oxygen-doped porous spiral carbon nanotubes, using spiral carbon nanotubes or spiral carbon nanotubes subjected to high-temperature carbonization as raw materials, preferentially removing the amorphous carbon part in the spiral carbon nanotubes by thermal oxidation, while the amorphous carbon part is oxidized and removed, forming a pore structure, and the carbon atoms around the pores are reconstructed and combined with oxygen atoms to form oxygen-containing functional groups.
[0040] The specific preparation steps include:
[0041] S1: using spiral carbon nanotubes or spiral carbon nanotubes treated by high temperature carbonization as raw materials;
[0042] S2: Place the raw material of S1 in a chamber of a thermal oxidation heating device with an oxygen or air atmosphere, raise the temperature to 400-600°C at 1-20°C / min, start the constant temperature program, and keep it for 0-1h to obtain a series of micro-meso-macroporous samples;
[0043] S3: Cool the series of micro-mesoporous and macroporous samples prepared in S2 to room temperature and then take them out.
[0044] The high-temperature carbonization treatment method of the spiral carbon nanotube raw material in S1 is to place the spiral carbon nanotube in an inert gas atmosphere such as nitrogen or argon, and heat it to above 700°C for carbonization treatment. The commonly used carbonization temperature is between 900°C and 1200°C.
[0045] In S2, the spiral carbon nanotubes or the spiral carbon nanotubes after high-temperature carbonization are placed in an oxygen-containing atmosphere such as air or oxygen, heated to 500° C. to 600° C. for thermal oxidation to form pores, and at the same time, oxygen atoms are doped into the carbon network around the pores.
[0046] The thermal oxidation heating device includes any one of a combustion heating device, a resistance heating device, an induction heating device, a microwave heating device and a radiation heating device.
[0047] An application of oxygen-doped porous helical carbon nanotubes, wherein the porous helical carbon nanotubes are applied to electromagnetic wave absorption and supercapacitors.
[0048] Example 2
[0049] Firstly, high-purity helical carbon nanotubes were grown on an alumina substrate carrying a Fe / Sn particle catalyst by CVD method, and high-purity helical carbon nanotubes were grown at a high temperature of 600-800°C under an argon protective atmosphere using acetylene as a carbon source.
[0050] Secondly, a certain amount of spiral carbon nanotubes were placed in a tube furnace and argon was introduced as a protective gas, with an argon flow rate of 400 sccm, and the temperature was raised to 1000°C at a heating rate of 5°C / min and maintained at this temperature for 1 hour. Figure 1 As shown in FIG. 1 , the surface of the pretreated helical carbon nanotubes is relatively smooth. The nitrogen adsorption-desorption curve of the above composite was tested using a BET instrument (BSD-PM1). Figure 5 As shown, its specific surface area is 17.7 m2 / g, and there are basically no micropores and mesopores.
[0051] Example 3
[0052] The control sample spiral carbon nanotubes in Example 2 were subjected to thermal oxidation treatment. The original spiral carbon nanotubes were directly transferred from the substrate carrying the carbon nanotubes, placed in a chamber of a heating device with an oxygen / air atmosphere, and heated to 500°C at 5 / min, and then the constant temperature program was started and maintained for 10 minutes to obtain a self-supporting oxygen-doped porous spiral carbon nanotube film that can be directly used for electrochemical measurement. Figure 2 As shown in FIG. 1 , the spiral carbon nanotubes have a small amount of defects and carbon wrinkles. The nitrogen adsorption and desorption curves of the above composites were tested using a BET instrument as shown in FIG. Figure 6 As shown, its specific surface area is 96.9m2 / g, and its pore size distribution is mainly concentrated at 0.86nm and 4.02nm. The oxygen content of the sample (Table 1) was tested by photoelectron spectroscopy (XPS, VG ESCALAB 250Xi) and was 4.45%, confirming that some oxygen atoms were incorporated into the carbon lattice.
[0053] Platinum sheet was selected as the counter electrode, mercuric oxide electrode as the reference electrode, and 6 mol / L KOH solution as the electrolyte. Electrochemical measurements were performed on the obtained oxygen-doped porous spiral carbon nanotube film self-supporting electrode on a CHI660E electrochemical workstation (Chenhua Instruments Inc.). Comparing the cyclic voltammetry (CV) test results of the original spiral carbon nanotube film self-supporting electrode and the oxygen-doped porous spiral carbon nanotube film self-supporting electrode, it can be seen that the voltage window of the spiral carbon nanotube film self-supporting electrode treated by thermal oxidation technology has been effectively broadened, such as Fig. 9 As shown in the figure, the specific capacitance value at the corresponding scan rate of 0.05V / s increased from 6.25F / g to 126.52F / g, which effectively improved the specific capacitance value at low current density; and the CV curve changed from an irregular shape to a rectangular shape, indicating that its energy storage mechanism is mainly surface-controlled double-layer capacitance, among which the redox peak at around ~0.7V can be attributed to the pseudocapacitance contributed by oxygen doping and carbon defects.
[0054] Example 4
[0055] The control sample spiral carbon nanotubes in Example 2 were subjected to thermal oxidation treatment. After the temperature of the heating chamber cooled to room temperature, it was raised to 500°C at 5°C / min in an air atmosphere, and then the constant temperature program was started and maintained at this temperature for 30 minutes. After the device was cooled naturally, oxygen-doped porous spiral carbon nanotube powder was obtained, such as Figure 3 As shown in FIG. 1 , the helical carbon nanotubes have many defects and wrinkles. The nitrogen adsorption and desorption curves of the above composites were measured using a BET instrument. Figure 7As shown, its specific surface area is 129.0m2 / g, and its pore size distribution is mainly concentrated at 0.76nm and 4.02nm. The oxygen content of the sample tested by photoelectron spectroscopy (Table 1) was further increased to 7.20%, confirming the increase in the amount of oxygen atom incorporation.
[0056] The wave absorption performance of the composite material was tested by a vector network analyzer. The oxygen-doped porous helical carbon nanotube powder was mixed with paraffin powder at a mass filling ratio of 3 wt.% to prepare a coaxial ring with an inner diameter of 3.04 mm, an outer diameter of 7.00 mm, and a thickness of 2.00 mm. The electromagnetic parameters of the sample were tested in the range of 1-18 GHz using a vector network analyzer (8720B, Agilent, USA), and the electromagnetic wave absorption curve was calculated and plotted according to the relevant formula, as shown in FIG. Fig.10 As shown in the figure, at a thickness of 2.2 mm, the effective absorption bandwidth of the sample is widened to 7.3 GHz, which is expected to be actually applied in absorbing materials.
[0057] Example 5
[0058] The control sample spiral carbon nanotubes in Example 2 were subjected to thermal oxidation treatment. After the temperature of the heating chamber cooled to room temperature, it was raised to 500°C at 5°C / min in an air atmosphere, and then the constant temperature program was started and maintained at this temperature for 50 minutes. After the device was cooled naturally, oxygen-doped porous spiral carbon nanotube powder was obtained, such as Figure 4 As shown in FIG. 1 , the helical carbon nanotubes have a large number of defects and wrinkles. The nitrogen adsorption and desorption curves of the above composites were measured using a BET instrument. Figure 8 As shown, its specific surface area is 187.2m2 / g, and its pore size distribution is mainly concentrated at 0.76nm and 3.8nm. The oxygen content of the sample was further tested using a photoelectron spectroscopy instrument (Table 1) and finally increased to 7.73%, achieving effective regulation of oxygen doping density.
[0059] The oxygen-doped porous helical carbon nanotube powder was mixed with paraffin powder at a mass filling ratio of 4 wt.%, and its wave absorbing performance was calculated according to the method described in Example 3. Fig.11 As shown, at a thickness of 2.2 mm, the effective absorption bandwidth of the sample is 7.1 GHz. This case confirms that the oxygen-doped porous helical carbon nanotubes in the present invention have broad application prospects in microwave absorption.
[0060] Oxygen-doped porous helical carbon nanotubes photoelectron spectroscopy analysis (content) Table 1:
[0061]
[0062] The working principle of the present invention is to preferentially remove the amorphous carbon part in the spiral carbon nanotube by a one-step thermal oxidation method. While the amorphous carbon part is oxidized and removed, a pore structure is formed, and the carbon atoms around the pores are reconstructed and combined with oxygen atoms to form oxygen-containing functional groups.
[0063] The present invention adopts thermal oxidation technology, combines defect engineering and microstructure design, and constructs a series of three-dimensional spiral carbon nanotube composite materials with defects and oxygen doping, and adjusts the density of defects and oxygen doping by controlling the oxidation time. Micropores and mesopores are formed at the same time, which greatly improves the specific surface area of spiral carbon nanotubes. The method is low-cost and easy to prepare, and the obtained oxygen-doped porous spiral carbon nanotubes have broad application prospects in the fields of energy storage, microwave absorption and electrochemical sensing.
[0064] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A porous helical carbon nanotube doped with oxygen, It is characterized in that With three-dimensional spiral carbon nanotubes as the skeleton, the thermal oxidation method is used to form pores on the three-dimensional spiral carbon nanotubes while doping oxygen atoms to form a porous material with a three-dimensional spiral chiral structure.
2. The oxygen-doped porous helical carbon nanotube according to claim 1, Features: The three-dimensional helical carbon nanotube is synthesized by chemical vapor deposition and has sp 2 and sp 3 Hybrid amorphous-polycrystalline structure.
3. A method for preparing oxygen-doped porous helical carbon nanotubes according to any one of claims 1 to 2, It is characterized in that Using spiral carbon nanotubes or spiral carbon nanotubes after high-temperature carbonization as raw materials, the amorphous carbon part in the spiral carbon nanotubes is preferentially removed by thermal oxidation. While the amorphous carbon part is oxidized and removed, a pore structure is formed. The carbon atoms around the pores are reconstructed and combined with oxygen atoms to form oxygen-containing functional groups.
4. The method for preparing oxygen-doped porous helical carbon nanotubes according to claim 3, It is characterized in that The specific preparation steps include: S1: using spiral carbon nanotubes or spiral carbon nanotubes treated by high temperature carbonization as raw materials; S2: Place the raw material of S1 in a chamber of a thermal oxidation heating device with an oxygen or air atmosphere, raise the temperature to 400-600°C at 1-20°C / min, start the constant temperature program, and keep it for 0-1h to obtain a series of micro-meso-macroporous samples; S3: Cool the series of micro-mesoporous and macroporous samples prepared in S2 to room temperature and then take them out.
5. The method for preparing oxygen-doped porous helical carbon nanotubes according to claim 4, Features: The high-temperature carbonization treatment method of the spiral carbon nanotube raw material in S1 is to place the spiral carbon nanotube in an inert gas atmosphere such as nitrogen or argon, and heat it to above 700°C for carbonization treatment. The commonly used carbonization temperature is between 900°C and 1200°C.
6. The method for preparing oxygen-doped porous helical carbon nanotubes according to claim 4, Features: In S2, the spiral carbon nanotubes or the spiral carbon nanotubes after high-temperature carbonization are placed in an oxygen-containing atmosphere such as air or oxygen, heated to 500° C. to 600° C. for thermal oxidation to form pores, and at the same time, oxygen atoms are doped into the carbon network around the pores.
7. The method for preparing oxygen-doped porous helical carbon nanotubes according to claim 4, Features: The thermal oxidation heating device includes any one of a combustion heating device, a resistance heating device, an induction heating device, a microwave heating device and a radiation heating device.
8. A use of the oxygen-doped porous helical carbon nanotube according to any one of claims 1 to 2, Features: The porous spiral carbon nanotube is applied to electromagnetic wave absorption and supercapacitor.
Citation Information
Patent Citations
Carbon nanotube, and preparation method and application thereof
CN104370279A
Preparation method and application of high-efficiency nitrogen-doped carbon nanotube
CN107686105A
Nitrogen-doped carbon nanotube particles, preparing method thereof, and supercapacitor electrode including the same
KR1020170093418A
Gyroidal mesoporous carbon materials and methods thereof
US20150041708A1
Cited By
Spiral carbon nanotube anode with controllable screw pitch, preparation method and application