Application of alcohol compounds in separation of semiconducting carbon nanotubes and method for separating semiconducting carbon nanotubes
By adding alcohol compounds to the carbon nanotube dispersion, the coating force of the polymer is changed, and the molecular force of the carbon nanotubes is used to separate metallic carbon nanotubes, which solves the problem of mixing metallic carbon nanotubes into semiconductor carbon nanotubes in the prior art. The problem of tubes has achieved high-purity semiconductor carbon nanotube separation, improving device performance.
Patent Information
- Application Number
- CN202410964356.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing carbon nanotube separation technology, the fluorenyl polymer does not have enough coating force on metallic carbon nanotubes, resulting in the mixing of metallic carbon nanotubes into semiconductor carbon nanotubes, affecting its purity and device performance.
Alcohol compounds are used to mix with mixed structure carbon nanotube dispersion containing semiconductor carbon nanotubes to change the solubility of the polymer, so that the polymer with weak coating strength is peeled off from the carbon nanotubes, and the carbon nanotubes are used. The molecular force agglomerates metallic carbon nanotubes, and improves the purity of semiconductor carbon nanotubes through centrifugation.
The purity of semiconductor carbon nanotubes is significantly improved, and the purity of semiconductor carbon nanotubes obtained by separation reaches more than 90%, reducing the influence of metal carbon tubes and improving the reliability of the device.
Smart Images

Figure HDA0004952442970000011 
Figure HDA0004952442970000012 
Figure HDA0004952442970000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon nanotube separation, and in particular relates to the application of alcohol compounds in separating semiconducting carbon nanotubes and a method for separating semiconducting carbon nanotubes. Background Art
[0002] Carbon materials have many different stable structures, such as diamond, graphene, carbon nanotubes and fullerenes. Among them, carbon nanotubes have been widely studied since they were first prepared in 1993. Single-walled carbon nanotubes are quasi-one-dimensional tubular materials that can be regarded as hollow cylinders formed by curling graphene. They usually have a diameter of nanometers to 10 nanometers and a length of several nanometers or even centimeters. Carbon nanotubes have broad application prospects in the fields of information, energy and biomedicine due to their excellent optical, electrical, thermal and mechanical properties. For example, metallic carbon nanotubes are ideal transparent conductive materials for the manufacture of flexible electronic devices due to their excellent conductivity, flexibility and stability, while semiconductor carbon nanotubes with nanometer-scale diameters have extremely high carrier mobility and a band gap that can be adjusted with the structure in device manufacturing, and can be used to manufacture high-performance, high-power-efficiency field-effect transistors. Carbon nanotubes can be used in many fields because they have a variety of structures with different atomic helicity, and different structures give them diverse physical properties.
[0003] The different structures of carbon nanotubes can be represented by a pair of integers (n, m), which specify the curling direction and degree of the carbon nanotubes. When the value of nm is a multiple of 3, the carbon nanotubes are metallic, and when the value of nm is not a multiple of 3, the carbon nanotubes are semiconducting. Therefore, among the carbon nanotubes whose structure growth is generally not controlled, about one-third are metallic tubes and two-thirds are semiconducting tubes. When carbon nanotubes are used in semiconductor devices, there are high requirements for the controllable structure and uniform performance of carbon nanotubes. For example, high-purity semiconductor carbon nanotubes can be used to prepare transistors with better performance than traditional silicon-based and other semiconductors. Therefore, it is difficult to directly use the mixed structure carbon nanotubes available on the market, and structural separation is required.
[0004] Existing carbon nanotube separation technologies include water-based separation and organic-based separation. Their separation principles are to use dispersants to specifically identify a certain type or class of carbon nanotubes to achieve separation. The existing fluorene-based polymer separation method can separate semiconductor carbon nanotubes in a mixed structure. Its advantages are high yield and efficient separation of large-diameter carbon nanotubes. The specific implementation is to mix carbon nanotubes and fluorene-based polymers in a toluene solvent, and ultrasonically crush the agglomerated carbon nanotubes to open them. After the polymer contacts the carbon nanotubes, it will specifically select and coat the surface of the semiconductor carbon nanotubes, while some semiconductor carbon tubes and metal carbon tubes that cannot be coated by the polymer will automatically agglomerate due to the intermolecular force. After centrifugation, the semiconductor carbon tubes that can be coated by the polymer can be dispersed in the supernatant, while the remaining carbon nanotubes that cannot be coated agglomerate and sink to the bottom, thereby achieving the separation of semiconductor carbon tubes.
[0005] However, the problem with the prior art is that the polymer does not have a strong enough resolution when selectively coating. When coating a small amount of metallic carbon nanotubes, the metallic carbon nanotubes are also mixed with the semiconductor carbon nanotubes and dispersed in the supernatant, which affects the purity of the separated semiconductor. In subsequent applications, this small amount of metallic carbon tubes will have a great impact on the device. For example, when used in integrated circuits, these small amounts of metallic carbon tubes will cause the device to short-circuit. Therefore, it is necessary to improve the purity of the fluorene-based polymer to separate the semiconductor carbon nanotubes. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide an application of an alcohol compound in separating semiconducting carbon nanotubes and a method for separating semiconducting carbon nanotubes. The application of an alcohol compound in separating semiconducting carbon nanotubes has simple operation and high purity.
[0007] The invention provides an application of an alcohol compound in separating semiconductor carbon nanotubes.
[0008] Preferably, the alcohol compound is a C1-C5 alcohol compound.
[0009] The present invention provides a method for separating semiconducting carbon nanotubes, comprising the following steps:
[0010] The alcohol compound and the mixed structure carbon nanotube dispersion containing the semiconductor carbon nanotube are mixed and centrifuged to obtain high-purity semiconductor carbon nanotubes.
[0011] Preferably, the mixed structure carbon nanotube dispersion containing semiconducting carbon nanotubes further comprises a solvent and a polymer;
[0012] The polymer is a fluorene-based polymer;
[0013] The solvent is one or more of toluene, chloroform, o-xylene, p-xylene and tetrahydrofuran.
[0014] Preferably, the alcohol compound is a C1-C5 alcohol compound.
[0015] Preferably, the volume ratio of the alcohol compound to the mixed-structure carbon nanotube dispersion containing semiconductor carbon nanotubes is (10-80) microliters: 1 mL.
[0016] Preferably, the centrifugal force used in the centrifugation is at least 4500 g, and the centrifugation time is more than 4 minutes.
[0017] Preferably, the mixed-structure carbon nanotube dispersion containing semiconductor carbon nanotubes also includes metallic carbon nanotubes.
[0018] Preferably, the alcohol compound and the mixed-structure carbon nanotube dispersion containing semiconductor carbon nanotubes are mixed, left to stand for 10 minutes to 30 days, and then centrifuged.
[0019] Preferably, the polymer is selected from one or more of poly[(9,9-dioctylfluorenyl-2,7-diyl)-alt-(6,6′-{2,2′-bipyridine})] (PFO-BPy), poly[9-(1-octyloyl)-9H-carbazole-2,7-diyl] (PCz), poly[(9,9-docosylfuranyl-2,7-diyl)] (PFDD) and poly(9,9-dioctylfluorene-2,7-diyl) (PFO), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylethynyl] (MEHPPV), poly[9,9-dihexylfluorene-2,7-diyl] (PFH), and poly(9,9-dioctylfluorene-altpyridine) (PFO-Py).
[0020] The present invention provides an application of an alcohol compound in separating semiconducting carbon nanotubes. In the present invention, a small amount of alcohol compound is added to a mixed structure carbon nanotube dispersion containing semiconducting carbon nanotubes. The alcohol compound changes the solubility of a polymer in a solvent such as toluene, thereby causing the polymer with a weaker coating force to peel off from the carbon nanotubes, that is, the polymer has a weaker coating force on metallic carbon nanotubes (on the contrary, the polymer has a stronger coating force on semiconducting carbon nanotubes). After losing the coating of the polymer, the exposed metallic carbon nanotubes will form agglomerations due to the strong molecular forces between the carbon nanotubes. After centrifugation, the metallic carbon nanotubes form precipitation at the bottom, thereby improving the purity of the semiconducting carbon nanotubes dispersed in the supernatant. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the process of separating semiconductor carbon nanotubes according to the present invention;
[0022] Figure 2 The spectrum test graphs of the preliminary dispersion prepared in Example 1 of the present invention and the dispersion after purification;
[0023] Figure 3 Spectral test graphs of the preliminary dispersion and the purified dispersion prepared in Example 2 of the present invention;
[0024] Figure 4 The spectrum test graphs of the preliminary dispersion liquid and the purified dispersion liquid prepared in Example 3 of the present invention;
[0025] Figure 5 The spectrum test graphs of the preliminary dispersion and the purified dispersion prepared in Example 4 of the present invention;
[0026] Figure 6 The spectrum test graphs of the preliminary dispersion and the purified dispersion prepared in Example 5 of the present invention;
[0027] Figure 7 Spectral test graphs of the preliminary dispersion and the purified dispersion prepared in Example 6 of the present invention;
[0028] Figure 8 Spectral test graphs of the preliminary dispersion and the purified dispersion prepared in Example 7 of the present invention;
[0029] Fig. 9 Spectral test graphs of the preliminary dispersion and the purified dispersion prepared in Example 8 of the present invention;
[0030] Fig.10 The spectrum test graphs of the preliminary dispersion prepared in Comparative Example 1 of the present invention and the dispersion after purification;
[0031] Fig.11 These are the spectrum test graphs of the preliminary dispersion prepared in Comparative Example 2 of the present invention and the dispersion after purification. DETAILED DESCRIPTION
[0032] The invention provides an application of an alcohol compound in separating semiconductor carbon nanotubes.
[0033] Materials such as alcohol compounds can improve the purity of polymer-separated semiconducting carbon nanotubes.
[0034] The alcohol compound described in the present invention is a C1-C5 alcohol compound.
[0035] The present invention provides a method for separating semiconducting carbon nanotubes, comprising the following steps:
[0036] The alcohol compound and the mixed structure carbon nanotube dispersion containing the semiconductor carbon nanotube are mixed and centrifuged to obtain high-purity semiconductor carbon nanotubes.
[0037] The present invention adopts alcohol compounds to improve the purity of fluorene-based polymers for separating semiconductor carbon nanotubes.
[0038] The alcohol compound in the present invention is a C1-C5 alcohol compound.
[0039] The dispersion containing the semiconducting carbon nanotubes in the present invention also includes metallic carbon nanotubes.
[0040] The dispersion containing the semiconducting carbon nanotubes in the present invention further comprises a solvent and a polymer;
[0041] The polymer is a fluorene-based polymer; preferably, the polymer is selected from one or more of poly[(9,9-dioctylfluorenyl-2,7-diyl)-alt-(6,6′-{2,2′-bipyridine})] (PFO-BPy), poly[9-(1-octyloyl)-9H-carbazole-2,7-diyl] (PCz), poly[(9,9-docosylfuranyl-2,7-diyl)] (PFDD) and poly(9,9-dioctylfluorene-2,7-diyl) (PFO), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylethynyl] (MEHPPV), poly[9,9-dihexylfluorene-2,7-diyl] (PFH), and poly(9,9-dioctylfluorene-altpyridine) (PFO-Py).
[0042] The solvent is one or more of toluene, chloroform, o-xylene, p-xylene and tetrahydrofuran.
[0043] In a specific embodiment of the present invention, the dispersion containing semiconducting carbon nanotubes is preferably prepared according to the following method:
[0044] The polymer and the solvent are mixed to obtain a polymer solution; the polymer solution is then mixed with mixed-structure carbon nanotubes containing semiconductor carbon nanotubes, ultrasonicated, and centrifuged to obtain a mixed-structure carbon nanotube dispersion containing semiconductor carbon nanotubes.
[0045] The hybrid carbon nanotubes containing semiconducting carbon nanotubes described in the present invention are commercially available products, such as AP-raw carbon nanotubes, Arc-discharge carbon nanotubes, CoMoCAT SG65 carbon nanotubes, CoMoCAT76 carbon nanotubes, Plasma carbon nanotubes, Tuball carbon nanotubes or HiPco carbon nanotubes.
[0046] The mass ratio of the polymer to the volume ratio of the solvent in the present invention is (5-10) mg:10 mL. The present invention adopts a heating method to dissolve the polymer in the solvent; specifically, a water bath heating method is adopted; the heating temperature is related to the type of polymer, and the heating temperature is preferably 50-70°C, more preferably 55-65°C; in a specific embodiment, the heating temperature is 60°C.
[0047] The mass ratio of the mixed carbon nanotubes containing semiconducting carbon nanotubes to the polymer is 1:10 to 10:1, preferably 2:1 to 1:2; in a specific embodiment, the mass ratio of the mixed carbon nanotubes containing semiconducting carbon nanotubes to the polymer is 3:5.
[0048] In the present invention, the polymer solution and the mixed carbon nanotubes containing the semiconductor carbon nanotubes are mixed and then ultrasonicated for 3 to 5 hours; more preferably, the ultrasonication is carried out under ice water bath conditions.
[0049] The present invention centrifuges the mixed solution obtained after ultrasonication to obtain a mixed structure carbon nanotube dispersion containing semiconductor carbon nanotubes; the centrifugal force used for centrifugation is at least 4500g, and the centrifugal time is more than 25 minutes. In a specific embodiment, the centrifugal force used for centrifugation is 4500g, and the centrifugal time is 30 minutes.
[0050] The present invention performs absorption spectrum test on the obtained mixed structure carbon nanotube dispersion containing semiconductor carbon nanotubes.
[0051] The present invention mixes an appropriate amount of a mixed structure carbon nanotube dispersion containing semiconductor carbon nanotubes and an alcohol compound; the volume ratio of the alcohol compound to the dispersion containing semiconductor carbon nanotubes is (10-80) microliters: 1 mL.
[0052] After mixing, it is preferably allowed to stand, so that the exposed carbon nanotube side walls are fully in contact with each other to form bundles. The larger the bundles are, the easier it is to precipitate them during subsequent centrifugation, so that they can be removed. The standing time is preferably 10 minutes to 20 hours. The alcohol compound is a C1 to C5 alcohol compound, specifically methanol, ethanol, isopropanol, etc.; in a specific embodiment, the alcohol compound is ethanol.
[0053] After standing, centrifuge the mixture, wherein the centrifugal force used for centrifugation is at least 4500g, and the centrifugal time is more than 4 minutes. In a specific embodiment, the centrifugal force used for centrifugation is 4500g, and the centrifugal time is 5 minutes.
[0054] The present invention performs absorption spectrum test on the purified dispersion containing semiconductor carbon nanotubes.
[0055] Figure 1 The steps for separating semiconducting carbon nanotubes in a specific embodiment of the present invention are as follows: a polymer: toluene solution is mixed with a mixed structure carbon nanotube, ultrasonically crushed, and centrifuged to obtain a semiconducting carbon nanotube dispersion (mixed with a small amount of metallic carbon nanotubes), a small amount of alcohol compound is added to the obtained supernatant, the mixture is allowed to stand, and centrifuged to obtain a high-purity semiconducting carbon nanotube dispersion and a metallic carbon nanotube precipitate.
[0056] In the present invention, a small amount of alcohol compounds is added to the dispersion containing semiconducting carbon nanotubes. The alcohol compounds will change the solubility of the polymer in the solvent such as toluene, thereby causing the polymer with weaker coating force to peel off from the carbon nanotubes, that is, the polymer has a weaker coating force on the metallic carbon nanotubes (on the contrary, the polymer has a stronger coating force on the semiconducting carbon nanotubes). After losing the coating of the polymer, the exposed metallic carbon nanotubes will form agglomerations due to the strong molecular forces between the carbon nanotubes. After centrifugation, the metallic carbon nanotubes will form a precipitate at the bottom, thereby improving the purity of the semiconducting carbon nanotubes dispersed in the supernatant.
[0057] To further illustrate the present invention, the application of the alcohol compounds provided by the present invention in separating semiconducting carbon nanotubes and the method for separating semiconducting carbon nanotubes are described in detail below in conjunction with the examples, but they should not be construed as limiting the scope of protection of the present invention.
[0058] Example 1
[0059] 5 mg of PFO-Bpy was added to 10 ml of toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 3 mg of AP-raw carbon nanotubes was added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0060] 2 ml of the solution after ultrasonic treatment was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 75%.
[0061] Take 1 ml of the above dispersion, add 40 microliters of ethanol, let it stand for 3 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test, the purity of the semiconductor carbon nanotubes is 99%.
[0062] Figure 2 These are the spectrum test graphs of the preliminary dispersion prepared in Example 1 of the present invention and the dispersion after purification.
[0063] Example 2
[0064] 5 mg of PFO-Bpy was added to 10 ml of toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 3 mg of AP-raw carbon nanotubes was added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0065] 2 ml of the solution after ultrasonic treatment was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 77%.
[0066] Take 1 ml of the above dispersion and add 20 μl, 40 μl, 60 μl and 80 μl of ethanol respectively. After standing for 3 hours, centrifuge at 4500*g for 5 minutes. Take the upper dispersion and perform absorption spectrum test. The purity of the semiconductor carbon nanotubes is 85%, 87%, 95% and 98% respectively.
[0067] Figure 3 These are the spectrum test graphs of the preliminary dispersion prepared in Example 2 of the present invention and the dispersion after purification.
[0068] Example 3
[0069] 5 mg of PFO-Bpy was added to 10 ml of toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 3 mg of AP-raw carbon nanotubes was added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0070] 2 ml of the solution after ultrasonic treatment was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 77%.
[0071] Take 1 ml of the above dispersion, add 80 μl of ethanol, let it stand for 0.5, 1, 3, 6, and 12 hours respectively, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test, the purity of the semiconductor carbon nanotubes is 83%, 90%, 95%, 97%, and 99% respectively.
[0072] Figure 4 These are the spectrum test graphs of the preliminary dispersion prepared in Example 3 of the present invention and the dispersion after purification.
[0073] Example 4
[0074] 5 mg PCZ was added to 10 ml toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 5 mg AP-raw carbon nanotubes were added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0075] 2 ml of the solution after ultrasonic treatment was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 89%.
[0076] Take 1 ml of the above dispersion, add 80 microliters of ethanol, let it stand for 3 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test, the purity of the semiconductor carbon nanotubes is 92%.
[0077] Figure 5 These are the spectrum test graphs of the preliminary dispersion and the purified dispersion prepared in Example 4 of the present invention.
[0078] Example 5
[0079] 5 mg PFDD was added to 10 ml toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 5 mg CoMoCAT76 carbon nanotubes were added to the solution, and the solution was ultrasonicated in an ice-water bath for 4 hours using an ultrasonic crushing device.
[0080] 2 ml of the sonicated solution was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 86%.
[0081] Take 1 ml of the above dispersion, add 80 microliters of ethanol, let it stand for 3 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test, the purity of the semiconductor carbon nanotubes is 91%.
[0082] Figure 6 These are spectral test graphs of the preliminary dispersion and the purified dispersion prepared in Example 5 of the present invention.
[0083] Example 6
[0084] 5 mg PCZ was added to 10 ml toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 5 mg Plasma carbon nanotubes were added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0085] 2 ml of the sonicated solution was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 83%.
[0086] Take 1 ml of the above dispersion, add 80 microliters of ethanol, let it stand for 3 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test, the purity of the semiconductor carbon nanotubes is 90%.
[0087] Figure 7These are the spectrum test graphs of the preliminary dispersion and the purified dispersion prepared in Example 6 of the present invention.
[0088] Example 7
[0089] 10 mg of PFO was added to 10 ml of toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 3 mg of HiPco carbon nanotubes was added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0090] 2 ml of the sonicated solution was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 88%.
[0091] Take 1 ml of the above dispersion, add 80 microliters of ethanol, let it stand for 18 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test, the purity of the semiconductor carbon nanotubes is 95%.
[0092] Figure 8 These are the spectrum test graphs of the preliminary dispersion prepared in Example 7 of the present invention and the dispersion after purification.
[0093] Example 8
[0094] 5 mg of PFO-Bpy was added to 10 ml of toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 3 mg of AP-raw carbon nanotubes was added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0095] 2 ml of the solution after ultrasonic treatment was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes. The dispersion was tested by absorption spectrum, and the purity of the semiconductor carbon nanotubes was 77%.
[0096] Take 1 ml of the above dispersion, add 40 microliters of isopropanol, let it stand for 3 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test, the purity of the semiconductor carbon nanotubes is 98%.
[0097] Fig. 9 These are the spectrum test graphs of the preliminary dispersion and the purified dispersion prepared in Example 8 of the present invention.
[0098] Comparative Example 1
[0099] 5 mg of PFO-Bpy was added to 10 ml of toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 3 mg of AP-raw carbon nanotubes was added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0100] 2 ml of the solution after ultrasonic treatment was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes, and the dispersion was subjected to absorption spectrum test;
[0101] Take 1 ml of the above dispersion, add 120 μl of ethanol, let it stand for 3 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test.
[0102] Fig.10 These are the spectrum test graphs of the preliminary dispersion prepared in Comparative Example 1 of the present invention and the dispersion after purification.
[0103] Comparative Example 2
[0104] 5 mg of PFO-Bpy was added to 10 ml of toluene, and the solution was heated at 60°C in a water bath to completely dissolve the polymer, thereby preparing a polymer: toluene solution. 3 mg of AP-raw carbon nanotubes was added to the solution, and the solution was sonicated in an ice-water bath using an ultrasonic crushing device for 4 hours.
[0105] 2 ml of the solution after ultrasonic treatment was taken and centrifuged at 4500*g for 30 min to obtain a preliminary dispersion of semiconductor carbon nanotubes mixed with a small amount of metallic carbon nanotubes, and the dispersion was subjected to absorption spectrum test;
[0106] Take 1 ml of the above dispersion, add 80 μl of ethanol, let it stand for 18 hours, then centrifuge it at 4500*g for 5 minutes, take the upper dispersion and perform absorption spectrum test.
[0107] Fig.11 These are the spectrum test graphs of the preliminary dispersion prepared in Comparative Example 2 of the present invention and the dispersion after purification.
[0108] As can be seen from the above embodiments, the present invention provides an application of alcohol compounds in separating semiconducting carbon nanotubes. In the present invention, a small amount of alcohol compounds is added to the dispersion containing semiconducting carbon nanotubes. The alcohol compounds will change the solubility of the polymer in the solvent such as toluene, so that the polymer with less strong coating force will be peeled off from the carbon nanotubes, that is, the polymer has a weaker coating force on the metallic carbon nanotubes (on the contrary, the polymer has a stronger coating force on the semiconducting carbon nanotubes). After losing the coating of the polymer, the exposed metallic carbon nanotubes will form agglomerations due to the strong molecular forces between the carbon nanotubes. After centrifugation, the metallic carbon nanotubes will form a precipitate at the bottom, thereby improving the purity of the semiconducting carbon nanotubes dispersed in the supernatant. The experimental results show that the purity of the separated semiconducting carbon nanotubes is more than 90%.
[0109] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Application of alcohol compounds in the separation of semiconducting carbon nanotubes.
2. The use according to claim 1, characterized in that: The alcohol compound is a C1-C5 alcohol compound.
3. A method for separating semiconductor carbon nanotubes, comprising the following steps: The alcohol compound and the mixed structure carbon nanotube dispersion containing the semiconductor carbon nanotube are mixed and centrifuged to obtain high-purity semiconductor carbon nanotubes.
4. The method according to claim 3, characterized in that: The dispersion containing the semiconducting carbon nanotubes also includes a solvent and a polymer; The polymer is a fluorene-based polymer; The solvent is one or more of toluene, chloroform, o-xylene, p-xylene and tetrahydrofuran.
5. The method according to claim 3, characterized in that: The alcohol compound is a C1 to C5 alcohol compound.
6. The method according to claim 5, characterized in that The volume ratio of the alcohol compound to the dispersion containing the semiconductor carbon nanotubes is (10-80) μL:1 mL.
7. The method according to claim 3, characterized in that The centrifugal force used in the centrifugation is at least 4500g, and the centrifugal time is more than 4 minutes.
8. The method according to claim 3, characterized in that The dispersion containing the semiconductor carbon nanotubes also includes metallic carbon nanotubes.
9. The method according to claim 3, characterized in that: The alcohol compound and the dispersion containing the semiconducting carbon nanotubes are mixed, left to stand for 10 minutes to 30 days, and then centrifuged.
10. The method according to claim 4, characterized in that The polymer is selected from one or more of poly[(9,9-dioctylfluorenyl-2,7-diyl)-alt-(6,6′-{2,2′-bipyridine})] (PFO-BPy), poly[9-(1-octyloyl)-9H-carbazole-2,7-diyl] (PCz), poly[(9,9-docosylfuranyl-2,7-diyl)] (PFDD) and poly(9,9-dioctylfluorene-2,7-diyl) (PFO), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylethynyl] (MEHPPV), poly[9,9-dihexylfluorene-2,7-diyl] (PFH), and poly(9,9-dioctylfluorene-altpyridine) (PFO-Py).