Graphene nanobelt preparation method based on nanowire mask printing process
Through the nanowire mask printing process, combined with electrohydraulic dynamic printing and plasma etching technology, the problems of complex process and uncertain morphology and size in the preparation of graphene nanoribbons are solved, and efficient and accurate preparation of graphene nanoribbons are achieved. , has promoted the development of nanotechnology.
Patent Information
- Application Number
- CN202411008377.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The existing graphene nanoribbon preparation method is complicated and the nanoribbon morphology cannot be accurately defined, which limits its feasibility for industrial-scale applications. In particular, the preparation technology of nanowire mask plates has uneven arrangement and pattern. Design problems.
Using nanowire mask printing technology, through electrohydraulic dynamic printing, plasma etching and ultrasonic peeling technology, polymethyl methacrylate solution is used to form a transferable film, accurately print organic polymer nanowires as masks, and pass Reactive ion etching technology removes graphene that is not covered by a mask, optimizing the width and spacing distribution of the nanoribbons.
The high horizontal and aspect ratio and one-dimensional structure of graphene nanoribbons have been achieved, which improves the controllability and consistency of preparation quality, simplifies the process flow, reduces costs, and provides the manufacturing of high-precision nanoelectronic devices. Strong technical support.
Smart Images

Figure CN118908192A_ABST
Abstract
Description
Technical field:
[0001] The invention belongs to the field of electronic devices, and in particular relates to a method for preparing graphene nanoribbons based on a nanowire mask printing process. Background technology:
[0002] In the context of the digital age, the rapid development of artificial intelligence technology is increasing the demand for advanced electronic devices. This trend has promoted the advancement of electronic material properties and manufacturing technologies in the fields of semiconductors and nanomaterials. As a two-dimensional nanomaterial, graphene has been widely studied for its excellent electronic properties with high carrier mobility, but its inherent property of zero bandgap manifests as a significant defect in some electronic applications, especially in semiconductor devices such as transistors.
[0003] The introduction of one-dimensional graphene nanoribbon technology provides an effective solution to the above problems. Through the quantum confinement effect caused by size reduction, the band gap of graphene nanoribbons has been expanded, giving it the functional characteristics of semiconductor materials. This characteristic transformation makes it possible to use graphene in electronic devices, especially in the manufacture of high-performance transistors. However, the current preparation methods of graphene nanoribbons usually use methods such as metal nanoparticle etching, carbon nanotube splitting, and atomic assembly, but these methods generally have complex processes and cannot accurately define the morphology and size of graphene nanoribbons, limiting their feasibility in industrial-scale applications. The method of using a one-dimensional mask for ion beam exposure can accurately control the width and morphology of graphene nanoribbons. However, the existing preparation technology of nanowire masks still has the challenge of uneven arrangement and distribution of nanowires and difficulty in customizing patterns. According to the document "Rational Fabrication of Graphene Nanoribbons Using a Nanowire Etch Mask" (see the American academic journal "Nano Letters" 2009, Vol. 9, pp. 2083-2087), chemically synthesized nanowires are used as mask plates in oxygen plasma etching to prepare graphene nanoribbons. However, the nanowire mask prepared by chemical synthesis cannot complete the design of precise mask patterns. According to the patent "A method for preparing graphene nanoribbons" (CN 110342504A, 2019.10.18), it is proposed that the probe manipulates the movement of the direction and distance of the nanowires, and finally the dispersed nanowires are arrayed, and the nanowire arrays are used as masks to etch the nanoribbons. However, this method requires manual adjustment of the direction and position of the nanowire mask, which is cumbersome and not conducive to the preparation of nanoribbon patterning of large-scale membranes. Summary of the invention:
[0004] The purpose of the present invention is to provide a method for preparing graphene nanoribbons based on nanowire mask printing process in view of the limitations of current technology. The method consists of electrohydrodynamic printing, plasma etching, and ultrasonic stripping technology. First, a polymethyl methacrylate (PMMA) solution is used to form a transferable film on the graphene surface, and then the copper foil at the bottom of the graphene is removed by ammonium persulfate etching. The digitally controllable nanowire technology is used to accurately print organic polymer nanowires on the graphene surface as a mask; the graphene not covered by the mask is accurately removed by reactive ion etching technology, and the mask is removed by ultrasonic stripping technology to obtain a one-dimensional graphene nanoribbon with a high aspect ratio. The present invention optimizes the width and spacing distribution of the graphene nanoribbon by carefully adjusting the key parameters such as the diameter, spacing and etching time of the nanowire mask, and improves the consistency and controllability of the preparation quality.
[0005] The technical solution of the present invention is:
[0006] A method for preparing graphene nanoribbons based on a nanowire mask printing process, the process steps of the method are as follows:
[0007] (1). Graphene film transfer:
[0008] The copper foil with the graphene film is attached to a glass sheet with isopropyl alcohol, and the PMMA solution is coated on the graphene surface by rotating at a low speed for 5-7 seconds and at a high speed for 40-60 seconds, and then dried at 70-80°C to form a PMMA / graphene / copper foil structure; then, the PMMA / graphene / copper foil is placed in an ammonium persulfate solution for 2-7 hours to etch off the copper foil substrate; after etching, the PMMA / graphene film is removed from the etching solution and washed in deionized water, and after washing, it is removed and dried on a Si / SiO2 substrate; then, it is placed in acetone, a mixed organic solvent and isopropyl alcohol in turn to remove PMMA; finally, the graphene film is dried at 85-90°C to obtain a graphene film transferred to a Si / SiO2 substrate;
[0009] The concentration of polymethyl methacrylate (PMMA) solution is 46-50 mg / mL, and each 4 cm 2 Silicon wafer coating 250-350μL;
[0010] The concentration of ammonium sulfate solution is 0.1-0.3 mol / L;
[0011] The low speed rotation is 1200-1500rpm / min; the high speed rotation is 3000-5000r / min;
[0012] The mixed organic solvent consists of acetone and isopropanol, and the volume ratio of the two is 1:1.
[0013] (2) Preparation for electrojet printing: Use vacuum adsorption to adsorb the substrate with graphene film on the substrate of the electrojet printing device; add the prepared precursor solution into the gas-tight syringe, adjust the distance between the bottom of the needle tube and the substrate surface to 2-3mm, and apply a bias voltage of 4000-4500V to the needle tube to form a single and stable nanowire jet;
[0014] The solute of the precursor solution is poly-9-vinyl carbazole, and the solvent is styrene; the concentration of poly-9-vinyl carbazole is 3-5wt%;
[0015] (3) Printing of nanowire arrays: Set the lateral movement distance of the printing substrate to 160-200 mm, the injection rate of the solution to 15-50 nL / min, the lateral movement speed to 50-260 mm / s, and the longitudinal movement speed to 0.6-2 mm / s, and start printing to obtain a nanowire array;
[0016] The diameter of the nanowires is 300-700 nm, the spacing of the nanowire arrays is 50-300 μm, and the length of the nanowires is 2.0-2.5 cm;
[0017] (4) Plasma etching: Place the substrate with the nanowire array printed in a plasma etcher, introduce oxygen as etching gas, with a gas flow rate of 80-100 sccm, a radio frequency power of 30-50 W, and an etching time of 20-40 s to remove the graphene not under the protection of the nanowires and obtain polymer / graphene nanoribbons;
[0018] (5) polymer removal: placing the polymer / graphene nanoribbon in an N,N-dimethylformamide solution, and removing the polymer on the graphene nanoribbon by ultrasonic treatment for 10-20 seconds to obtain the graphene nanoribbon attached to the substrate;
[0019] Also included are the substrate pre-treatment steps:
[0020] Substrate cleaning: First, the Si / SiO2 substrate is cut and ultrasonically cleaned; the cleaning process includes cleaning in deionized water for 15-20 minutes, then cleaning in an acetone solution for 20-30 minutes, and finally treating in an isopropanol solution for 15-20 minutes.
[0021] Substrate treatment: Use a nitrogen gun to blow dry the cleaned substrate surface, and then place the substrate in an ozone cleaning machine for 20-30 minutes to improve the surface activity of the substrate.
[0022] The graphene nanoribbon prepared by the method is used as a conductive channel layer of a three-terminal structure transistor device.
[0023] The essential features of the present invention are:
[0024] Traditional methods for preparing graphene nanoribbons usually require complex steps, such as nanoparticle deposition in metal nanoparticle erosion, high-precision cutting in carbon nanotube dissection, and layer-by-layer construction in atomic assembly, etc. The process is cumbersome and time-consuming. The present invention only requires steps such as electrohydrodynamic printing, plasma etching and ultrasonic peeling, which simplifies the process;
[0025] The method uses controllable digital nanowire printing technology to print a poly 9-vinyl carbazole nanowire mask on the graphene surface, and uses reactive ion etching technology to etch away the graphene not protected by the nanowire mask to prepare graphene nanoribbons. During the preparation process, the width and spacing of the graphene nanoribbons are regulated by changing the diameter of the poly 9-vinyl carbazole nanowire mask, the nanowire spacing, and the oxygen plasma etching time, thereby regulating the electrical properties of the graphene nanoribbons.
[0026] The method adopted by the present invention realizes large-area, rapid and low-cost preparation of graphene nanoribbons, as well as precise regulation of the width and spacing of graphene nanoribbons, providing a basis for opening the graphene band gap and constructing graphene nanoribbon-based electronic devices.
[0027] The beneficial effects of the present invention are:
[0028] (1) The digitally controllable nanowire printing technology used in the present invention can print a one-dimensional polymer nanowire mask with uniform width and spacing on the graphene surface by precisely adjusting printing parameters such as bias voltage, printing distance, printing speed and pattern parameters. The core advantage of this technology is that it has a high degree of controllability and flexibility compared with the existing graphene nanoribbon preparation technology. At the same time, the pattern of the nanowire can be freely customized as needed, providing strong technical support for the preparation of high-precision nanoelectronic devices.
[0029] (2) The plasma etching technology used in the present invention can precisely control the width and spacing of graphene nanoribbons while maintaining the integrity of the morphology by adjusting the diameter of the nanowire mask and the etching time. This allows the adjustment of the energy band width of the nanoribbons and realizes the applicability of graphene nanoribbons in transistor devices. In addition, this technology also provides new methods and ideas for the manufacture of one-dimensional structures of other similar nanomaterials, promoting the development of nanotechnology and related technical fields.
[0030] (3) Compared with photolithography and other nanobelt preparation methods, the present invention has obvious advantages in manufacturing cost and efficiency. Digitally controllable nanowire printing technology avoids the use of expensive mask plates and photoresists and can also achieve patterned mask printing; the automated printing process greatly reduces the complexity of process operations; 2Only 1 to 10 μL of solution is required to complete one print on a silicon wafer of a certain size, which reduces the amount of material used in the production process and achieves high-precision and high-efficiency nanoribbon production. Description of the drawings:
[0031] Figure 1 Schematic diagram of the process of preparing graphene nanoribbons by plasma etching and cleaning for printing nanowire masks on graphene.
[0032] Figure 2 This is a characterization image of a single poly-9-vinylcarbazole nanowire mask printed on a graphene film using a digitally controllable nanowire printer in Example 1 under an optical microscope at 100 times magnification.
[0033] Figure 3 This is a characterization image of the poly 9-vinylcarbazole nanowire array printed on the graphene film using the digitally controllable nanowire printer in Example 1 under an optical microscope at 20 times magnification.
[0034] Figure 4 This is a characterization image of a single graphene nanoribbon obtained after removing the nanowire mask by plasma etching and ultrasonic cleaning in Example 1 under an optical microscope at 100 times magnification;
[0035] Figure 5 This is a characterization image of the graphene nanoribbon array obtained after removing the nanowire mask by plasma etching and ultrasonic cleaning in Example 1 under an optical microscope at 10 times magnification;
[0036] Figure 6 This is a scanning electron microscope image of a single graphene nanoribbon in Example 1 at a magnification of 100,000;
[0037] Figure 7 This is a characterization image of a single graphene nanoribbon in Example 1 under an atomic force microscope.
[0038] Figure 8 This is the transfer characteristic curve of the graphene nanoribbon device in Example 1.
[0039] Among them, 1 is a Si / SiO2 substrate, 2 is a graphene film, 3 is a poly-9-vinylcarbazole nanowire mask, and 4 is a graphene nanoribbon after plasma etching and N,N-dimethylformamide ultrasonic removal of the polymer nanowire mask.
[0040] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments: Specific implementation plan:
[0041] like Figure 1As shown, the left side of the picture shows that the PVK nanowire array mask (3) is evenly printed on the graphene film 2 transferred to the Si / SiO2 substrate 1. The middle part of the figure shows the oxygen plasma (O + ) The graphene film not covered by the PVK nanowire array mask is etched to react with CO2 gas to escape. The right side of the picture shows the graphene nanoribbon 4 obtained after the etching is completed and the PVK nanowire mask is removed by DMF ultrasonic cleaning. The specific implementation plan is as follows:
[0042] Embodiment 1:
[0043] (1) Cut the silicon wafer substrate with SiO2 oxide layer into 2×2 cm 2 Size, put it in deionized water and use ultrasonic cleaning instrument to ultrasonically clean it for 15 minutes, then pour out the deionized water and add acetone solution, and ultrasonically clean it for 30 minutes. Finally, pour out the acetone and add isopropanol solution, and ultrasonically treat it for 15 minutes to complete the cleaning of Si / SiO2 substrate. Use nitrogen gun to blow dry the surface of the cleaned substrate, and then place the substrate in ozone cleaning machine for ozone treatment for 30 minutes to improve the surface activity of the substrate.
[0044] (2) Cut the copper foil (50 μm thick) with 0.35 nm thick graphene film into 1.5 × 1.5 cm 2 The size of the copper foil was attached to a clean glass sheet by isopropanol. PMMA solution (solution concentration was 46 mg / mL, solvent was chlorobenzene) was spin-coated on the graphene surface, and the spin-coating parameters were low speed 1500 rpm / min for 5 seconds and high speed 3000 rpm / min for 60 seconds. The PMMA / graphene / copper foil structure was then transferred to a heating table and dried at 70°C.
[0045] (3) Peel the PMMA / graphene / copper foil off the glass sheet and immerse it in an ammonium persulfate solution (0.2 mol / L, 400 mL) to etch the copper foil substrate for 4 h, so that the PMMA / graphene film floats on the surface of the etching solution. Remove the PMMA / graphene film from the etching solution, wash it with deionized water, and transfer it to a Si / SiO2 substrate to dry. Place it in acetone, acetone: isopropanol = 1:1 (volume ratio), and isopropanol reagent in turn to remove PMMA. Finally, dry the graphene film at 90°C to successfully achieve the transfer of graphene to the Si / SiO2 substrate.
[0046] (4) Take 40 mg of poly-9-vinyl carbazole and 1 g of styrene, and stir them with a magnetic rotor at room temperature and pressure. The stirring speed is 500 rpm, and the stirring time is 4 hours until the poly-9-vinyl carbazole is completely dissolved, and the color of the dissolved precursor solution is colorless and transparent.
[0047] (5) The substrate with the graphene film is adsorbed onto the substrate of the electrofluidic printing device by vacuum adsorption. The prepared precursor solution is added to a gas-tight syringe with a syringe needle having an outer diameter of 240 μm and an inner diameter of 60 μm. The injection rate of the solution is set to 15 nL / min. The distance between the bottom of the needle and the substrate surface is adjusted to 2 mm, and a single and stable nanowire jet is formed by applying a bias voltage of 4000 V to the needle. The lateral movement distance of the printed substrate is set to 180 mm, the lateral movement speed is 50 mm / s, and the longitudinal movement speed is 0.6 mm / s. In the obtained nanowire array, the diameter of the nanowire is 400 nm, the nanowire array spacing is 100 μm, and the length of the nanowire is 2.0 cm. The substrate temperature is adjusted to 35 ° C and the substrate is heated for 5 minutes. The substrate can be removed without destroying the nanowires on the substrate.
[0048] (6) Place the substrate with the nanowire array printed in a plasma etcher. Use oxygen as etching gas, with a gas flow rate of 80 sccm, a radio frequency power of 30 W, and an etching time of 20 s to remove the graphene not under the nanowires and obtain polymer / graphene nanoribbons.
[0049] (7) The polymer / graphene nanoribbon is placed in an N,N-dimethylformamide solution, and the PVK nanowire array mask on the graphene nanoribbon is removed by ultrasonic treatment for 20 seconds. After the ultrasonic treatment, the residual liquid is blown dry with a small amount of N2 gas flow to obtain the graphene nanoribbon attached to the substrate.
[0050] (8) 0.5 g of gold wire was taken as an evaporation source, and a source-drain electrode with a thickness of 50-80 nm was deposited on the graphene nanoribbon by evaporation deposition technology. A cross-finger electrode mask was selected, and the interdigital spacing of the mask was 100 μm.
[0051] Figure 2 and Figure 3 This is an optical microscope image of the nanowire array prepared on the graphene nanoribbon by electrofluidic printing technology in Example 1. It can be seen that the printed nanowire array is evenly arranged, the spacing between the nanowires is about 100 μm, and the diameter is about 300 nm.
[0052] Figure 4 and Figure 5 Optical microscope image of graphene nanoribbon array after plasma etching and ultrasonic removal of nanowire mask. Figure 4 The graphene nanoribbon morphology observed at 100 times magnification. Figure 5The prepared nanoribbon array was photographed at 10 times magnification, which includes graphene nanoribbons and the part where the graphene film is not transferred on the substrate. It can be clearly seen that after the etching and cleaning process, the nanowires in the part where the graphene is not transferred on the substrate have been completely removed, and the remaining graphene nanoribbon array also retains excellent surface morphology and uniformity, which also confirms the feasibility of the process.
[0053] Figure 6 This is a scanning electron microscope image of a single graphene nanoribbon obtained in Example 1 at 100,000 times magnification. The width of the nanoribbon is uniform, about 250 nm.
[0054] Figure 7 This is an atomic force microscope characterization image of a single graphene nanoribbon obtained in Example 1. The upper right curve is the nanoribbon height curve at the line connecting two points AB. It can be seen that the height of the nanoribbon is 2.8 nm.
[0055] Figure 8 This is the transfer characteristic curve of the graphene nanoribbon transistor device measured by the instrument Keithley 4200A, where the current changes with the gate voltage. The test range is -60V to 60V. The transfer characteristic curve of the graphene nanoribbon device shows the nonlinear characteristics of the hysteresis effect. The nonlinear characteristics indicate that the transistor can be turned on and off accurately by adjusting the gate voltage, thereby achieving more flexible threshold voltage control. Within a certain gate voltage range, the nonlinear characteristics can provide higher gain and achieve effective signal amplification. The hysteresis effect indicates that the current-voltage characteristics of the transistor are path-dependent and have a memory effect.
[0056] Embodiment 2:
[0057] (1) Cut the silicon wafer substrate with SiO2 oxide layer into 2×2 cm 2 Size, put it in deionized water and use ultrasonic cleaning instrument to ultrasonically clean it for 15 minutes, then pour out the deionized water and add acetone solution, and ultrasonically clean it for 30 minutes. Finally, pour out the acetone and add isopropanol solution, and ultrasonically treat it for 15 minutes to complete the cleaning of Si / SiO2 substrate. Use nitrogen gun to blow dry the surface of the cleaned substrate, and then place the substrate in ozone cleaning machine for ozone treatment for 30 minutes to improve the surface activity of the substrate.
[0058] (2) Prepare ammonium persulfate solution (0.2 mol / L) for etching the copper foil substrate and PMMA solution (46 mg / mL) for preparing the support layer. Cut the copper foil (50 μm thick) with a 0.35 nm thick graphene film into 1.5×1.5 cm 2The size of the copper foil was attached to a clean glass sheet by isopropanol solution. PMMA solution (46 mg / mL) was spin-coated on the graphene surface with the spin-coating parameters of 1500 rpm / min for 5 s and 3000 rpm / min for 60 s. The PMMA / graphene / copper foil structure was obtained by drying on a heating table at 70°C.
[0059] (3) Peel PMMA / graphene / copper foil off the glass sheet and immerse it in ammonium persulfate solution (0.2 mol / L, 400 mL) to etch the copper foil substrate. Use ammonium persulfate solution to etch the copper foil substrate so that the PMMA / graphene film floats on the surface of the etching solution. Remove the PMMA / graphene film from the etching solution, wash it with deionized water, and transfer it to the Si / SiO2 substrate to dry. Place it in acetone, acetone: isopropanol = 1:1, and isopropanol reagent in turn to remove PMMA. Finally, dry the graphene film at 90°C to successfully achieve the transfer of graphene to the Si / SiO2 substrate.
[0060] (4) Take 40 mg of poly-9-vinyl carbazole and 1 g of styrene, and stir them with a magnetic rotor at room temperature and pressure. The stirring speed is 500 rpm, and the stirring time is 4 hours until the poly-9-vinyl carbazole is completely dissolved, and the color of the dissolved precursor solution is colorless and transparent.
[0061] (5) The substrate with the graphene film is adsorbed onto the substrate of the electrofluidic printing device by vacuum adsorption. The prepared precursor solution is added to a gas-tight syringe with a syringe needle having an outer diameter of 300 μm and an inner diameter of 160 μm. The injection rate of the solution is set to 50 nL / min. The distance between the bottom of the needle and the substrate surface is adjusted to 2.5 mm, and a single and stable nanowire jet is formed by applying a bias voltage of 4500 V to the needle. The lateral movement distance of the printed substrate is set to 180 mm, the lateral movement speed is 260 mm / s, and the longitudinal movement speed is 0.6 mm / s. In the obtained nanowire array, the diameter of the nanowire is 700 nm, the nanowire array spacing is 100 μm, and the length of the nanowire is 2.0 cm. The substrate temperature is adjusted to 35 ° C and the substrate is heated for 5 minutes. The substrate can be removed without destroying the nanowires on the substrate.
[0062] (6) Place the substrate with the nanowire array printed in a plasma etcher. Use oxygen as etching gas, with a gas flow rate of 80 sccm, a radio frequency power of 30 W, and an etching time of 40 s to remove the graphene not under the nanowires and obtain polymer / graphene nanoribbons.
[0063] (7) placing the polymer / graphene nanoribbon in an N,N-dimethylformamide solution, and removing the polymer on the graphene nanoribbon by ultrasonic treatment for 20 seconds. After the ultrasonic treatment, the remaining liquid is blown dry with a small amount of N2 gas flow to obtain the graphene nanoribbon.
[0064] (8) 0.5 g of gold wire was taken as an evaporation source, and a source-drain electrode with a thickness of 50-80 nm was deposited on the graphene nanoribbon by evaporation deposition technology. A cross-finger electrode mask was selected, and the interdigital spacing of the mask was 100 μm.
[0065] From the above examples, it can be seen that the present invention successfully achieves the one-dimensional patterning preparation requirements for graphene nanoribbons by combining the two processes of electrohydrodynamic printing and plasma etching. In this process, EHD printing is used for precise deposition of the protective layer, which ensures high precision and uniformity of the pattern. The area not covered by the protective material is then removed by an etching step, thereby accurately forming the desired specific patterned nanostructure.
[0066] The graphene nanoribbon prepared by the present invention has significant one-dimensional characteristics. The measured transfer characteristic curve data show that the switching ratio of the graphene nanoribbon transistor is about 12, which is higher than that of the traditional graphene material without band gap (usually the switching ratio is between 1 and 2), indicating that the nanoribbon structure prepared by the process method can successfully introduce a band gap. In addition, Figure 8 The nonlinear part (-60V to 60V) of the IV transfer characteristic curve shown in the figure shows that the electrical properties of graphene nanoribbons exhibit semiconductor material properties that are different from conductors. In addition, Figure 8 The IV transfer characteristic curves of the positive and negative scans shown do not overlap, demonstrating the field effect control capability of the hysteresis effect similar to that of the field effect transistor and the characteristics of the semiconductor material, opening up a new path for the manufacture of high-performance electronic devices.
[0067] Matters not covered by the present invention are known technologies.
Claims
1. A method for preparing graphene nanoribbons based on a nanowire mask printing process, wherein the process steps of the method are as follows: (1). Graphene film transfer: The copper foil with the graphene film is attached to a glass sheet with isopropyl alcohol, and the PMMA solution is coated on the graphene surface by rotating at a low speed for 5-7 seconds and at a high speed for 40-60 seconds, and then dried at 70-80°C to form a PMMA / graphene / copper foil structure; then, the PMMA / graphene / copper foil is placed in an ammonium persulfate solution for 2-7 hours to etch away the copper foil substrate; After etching, the PMMA / graphene film is removed from the etching solution and washed in deionized water, and then removed and dried using a Si / SiO2 substrate; then, the PMMA is removed by sequentially placing the film in acetone, a mixed organic solvent, and isopropanol; finally, the graphene film is dried at 85-90°C to obtain a graphene film transferred to the Si / SiO2 substrate; Wherein, the concentration of polymethyl methacrylate (PMMA) solution is 46-50 mg / mL; (2) Preparation for electrojet printing: Use vacuum adsorption to adsorb the substrate with graphene film on the substrate of the electrojet printing device; add the prepared precursor solution into the gas-tight syringe, adjust the distance between the bottom of the syringe and the substrate surface to 2-3mm, set the injection rate of the solution to 15-50nL / min, and apply a bias voltage of 4000-4500V to the syringe to form a single and stable nanowire jet; The solute of the precursor solution is poly-9-vinyl carbazole, the solvent is styrene, and the concentration of poly-9-vinyl carbazole is 3-5wt%; (3) Printing of nanowire arrays: Set the lateral movement distance of the printing substrate to 160-200 mm, the lateral movement speed to 50-260 mm / s, and the longitudinal movement speed to 0.6-2 mm / s, and start printing to obtain a nanowire array; The diameter of the nanowires is 300-700 nm, the spacing of the nanowire arrays is 50-300 μm, and the length of the nanowires is 2.0-2.5 cm; (4) Plasma etching: Place the substrate with the nanowire array printed in a plasma etcher, introduce oxygen as etching gas, with a gas flow rate of 80-100 sccm, a radio frequency power of 30-50 W, and an etching time of 20-40 s to remove the graphene not under the protection of the nanowires to obtain polymer / graphene nanoribbons; (5) Polymer removal: The polymer / graphene nanoribbon is placed in an N,N-dimethylformamide solution, and the polymer on the graphene nanoribbon is removed by ultrasonic treatment for 10-20 seconds to obtain a graphene nanoribbon attached to the substrate.
2. The method for preparing graphene nanoribbons based on nanowire mask printing process according to claim 1, characterized in that The pretreatment step of the substrate in step (1): Substrate cleaning: First, the Si / SiO2 substrate is cut and ultrasonically cleaned; the cleaning process includes cleaning in deionized water for 15-20 minutes, then cleaning in an acetone solution for 20-30 minutes, and finally treating in an isopropanol solution for 15-20 minutes. Substrate treatment: Use a nitrogen gun to blow dry the cleaned substrate surface, and then place the substrate in an ozone cleaning machine for 20-30 minutes to improve the surface activity of the substrate.
3. The method for preparing graphene nanoribbons based on nanowire mask printing process as described in claim 1, characterized in that the concentration of ammonium sulfate solution is 0.1-0.3 mol / L; the mixed organic solvent consists of acetone and isopropanol, and the volume ratio of the two is 1:
1.
4. The method for preparing graphene nanoribbons based on nanowire mask printing process according to claim 1, characterized in that every 4 cm 2 The silicon wafer is coated with 250-350 μL.
5. The method for preparing graphene nanoribbons based on nanowire mask printing process as described in claim 1, characterized in that the low-speed rotation is 1200-1500 rpm / min; the high-speed rotation is 3000-5000 r / min.
6. The application of the graphene nanoribbon prepared by the method as claimed in claim 1, characterized in that Used as the conductive channel layer of a three-terminal transistor device.
Citation Information
Patent Citations
Preparation method of one-dimensional scale limited graphene nano band
CN102254795A
Graphene nano-belts, preparation method of graphene nano-belts, and application of graphene nano-belts in transparent electrodes
CN103848415A