Preparation method of phenolic resin-based porous carbon spheres

Phenolic resin microspheres were prepared by batch low-speed dropwise addition and high-speed stirring. Combined with sintering and activation treatment, the monodispersity and particle size inhomogeneity of phenolic resin-based porous carbon spheres were solved, and porous carbon spheres with high specific surface area and uniform particle size were prepared, thus improving the material performance.

CN118908209APending Publication Date: 2024-11-08郑州坚峰复合材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410881874.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies for preparing phenolic resin-based porous carbon spheres suffer from poor monodispersity, easy particle agglomeration, and low specific surface area.

Method used

Phenolic resin microspheres were prepared by batch low-speed dropwise addition and high-speed stirring. Combined with sintering and activation treatment, the reaction rate and temperature were controlled to ensure the dispersibility and particle size uniformity of the phenolic resin microspheres, forming a porous structure.

Benefits of technology

Phenolic resin-based porous carbon spheres with high specific surface area and uniform particle size were prepared, which improved the material's performance and application effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908209A_ABST
    Figure CN118908209A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of phenolic resin-based porous carbon spheres. The preparation method comprises the following steps: taking a phenol source, a dispersing agent, formaldehyde, a stabilizing agent, an activating agent and a catalyst as main raw materials, synthesizing phenolic resin-based microspheres at normal temperature, and then carbonizing and activating to obtain the phenolic resin-based porous carbon spheres. The phenolic resin-based porous carbon spheres prepared by the method are high in monodispersity, free of adhesion, high in specific surface area, short in reaction time, high in production efficiency, environmentally friendly, free of pollution and beneficial to large-scale production, and solvents such as alcohols are not needed in the preparation process, and high temperature and high pressure are not needed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of special structure carbon materials, and in particular relates to a method for preparing phenolic resin-based porous carbon spheres. Background Art

[0002] Phenolic resin-based porous carbon balls are a kind of lightweight spherical porous material with strong adsorption capacity. They are widely used in military industry, medicine and new energy fields.

[0003] In the existing preparation technology of phenolic resin-based porous carbon spheres, there are often problems such as poor monodispersity, easy agglomeration of particles, and low specific surface area, which affect the performance of phenolic resin-based porous carbon spheres. Summary of the invention

[0004] The purpose of the present invention is to provide a method for producing resin-based porous carbon spheres with high specific surface area and uniform particle size.

[0005] The technical solution adopted by the present invention is a method for preparing phenolic resin-based porous carbon spheres, which is specifically implemented according to the following steps:

[0006] A phenol source, a dispersant and water are mixed to prepare a mixed solution A; formaldehyde, a stabilizer and a catalyst are mixed to prepare a mixed solution B;

[0007] Divide the mixed solution B into at least two portions, and add one portion of the mixed solution B dropwise into the mixed solution A each time, and mix and stir at a high speed until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C;

[0008] Drying the mixed solution C to obtain phenolic resin microspheres;

[0009] sintering the phenolic resin microspheres to obtain phenolic resin-based carbon spheres;

[0010] An activator is added to phenolic resin-based carbon spheres, and the phenolic resin-based porous carbon spheres are obtained by grinding and sintering.

[0011] In this way, the mixed solution B is slowly added to the mixed solution A in multiple times, so that the reaction rate of the mixed solution B and the mixed solution A is slowed down, and the uneven reaction caused by the simultaneous reaction of large doses of the mixed solution A and the mixed solution B is avoided, so that the dispersant in the mixed solution A can fully play a role in the reaction process, and at the same time, through high-speed stirring, the prepared phenolic resin microspheres can be prevented from sticking to each other, thereby improving the dispersibility and uniformity of the phenolic resin microsphere particles. Among them, the steric hindrance effect of the dispersant has a dispersing effect on the microspheres, inhibiting the adhesion of the phenolic microspheres, narrowing the particle size distribution, and the dispersant can also promote uniform nucleation of the spheres by changing the surface tension of the droplets, thereby obtaining a smaller microsphere size.

[0012] In some embodiments, the mixed solution B is divided into at least two portions, and one portion of the mixed solution B is added dropwise into the mixed solution A each time and mixed and stirred until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C. The process also includes that each time the mixing is performed, the dropping speed of the mixed solution B is 40 to 60 drops / min, and the mixing and stirring temperature is 15°C to 35°C.

[0013] Thus, the mixed solution B and the mixed solution A are slowly mixed and reacted at room temperature, so that the generated phenolic resin microspheres have dispersion and uniformity. The mixing and stirring temperature is 15°C to 35°C to control the reaction speed, avoiding the microspheres from sticking together and uneven particle size due to too fast reaction or the production efficiency from being affected by too slow reaction.

[0014] In some embodiments, the mixed solution B is divided into at least two portions, and one portion of the mixed solution B is added dropwise into the mixed solution A each time for mixing and stirring, which also includes dividing the mixed solution B into n portions, and the mixed solution B added for the first time is recorded as B1, and the second, third, ..., nth times are recorded as B2, B3, ..., Bn respectively, wherein B:B1=1:(1 / 6~1 / 2), and B2~Bn are equally divided.

[0015] Thus, a portion of mixed solution B is added first to react with mixed solution A. Since heat is released when the phenol source and formaldehyde are synthesized into phenolic resin, if the reaction between the two is too intense, a large amount of heat will be released, causing the reaction temperature to get out of control, thereby further polymerizing the synthesized phenolic resin microspheres, increasing the particle size or causing adhesion. The equal portions of B2 to Bn are used to further control the reaction speed, make the reaction proceed as uniformly as possible, and improve the reaction efficiency as much as possible under the premise of sufficient reaction, so as to obtain phenolic resin microspheres with uniform particle size.

[0016] Preferably, the high-speed mixing and stirring is carried out using a reactor with a rotation speed of 150-300 r / min.

[0017] In this way, high-speed stirring allows the reactants to react uniformly while the generated phenolic resin microspheres have a monodisperse characteristic.

[0018] In some embodiments, the mass ratio of phenol source, dispersant, water, formaldehyde, catalyst and stabilizer is (10-30):(1-3):(100-200):(3-18):(6-20):1;

[0019] In some embodiments, the phenol source is selected from one or more of p-aminophenol, m-aminophenol, o-aminophenol, resorcinol, catechol, hydroquinone, and phloroglucinol;

[0020] In some embodiments, the dispersant is selected from one or more of Tween 80, Tween 60, polyvinyl alcohol, polypyrrolidone, polyethylene glycol, sodium dodecyl sulfonate, sodium dodecyl sulfate, hexadecyl ammonium bromide, OP-30, and triblock copolymer F127;

[0021] In some embodiments, the stabilizer is selected from one or more of salicylic acid, sodium salicylate, 4-amino-2-hydroxybenzoic acid, phloroglucinolcarboxylic acid, 2,4-dihydroxybenzoic acid, and 3,5-dihydroxybenzoic acid;

[0022] In some embodiments, the catalyst is selected from one or more of ammonia, triethylamine, sodium hydroxide, potassium hydroxide, barium hydroxide, magnesium hydroxide, and sodium carbonate;

[0023] In some embodiments, the sintering process for preparing phenolic resin-based carbon spheres is to first heat the temperature to 180-250° C. and hold for 0.5-1 h, then heat the temperature to 400-800° C. and hold for 1-2 h;

[0024] In some embodiments, the activator is selected from one or more of sodium hydroxide, potassium hydroxide, calcium chloride, and zinc chloride;

[0025] In some embodiments, the amount of the activator is 2 to 4 times the mass of the phenolic resin-based carbon spheres;

[0026] In some embodiments, the grinding time after adding the activator to the phenolic resin-based carbon spheres is 0.5 h to 1 h;

[0027] In some embodiments, the sintering process for preparing phenolic resin-based porous carbon spheres is to first heat the temperature to 400-450° C. and maintain it for 0.5-1 h, then heat the temperature to 600-800° C. and maintain it for 1-3 h, and finally cool it to room temperature in the furnace.

[0028] The invention uses high-speed stirring and batch low-speed dripping to make mixed solution A and mixed solution B react uniformly, so that the prepared phenolic resin microspheres have high dispersibility, do not adhere to each other, and have uniform particle sizes. The reaction process of the mixed solution A and the mixed solution B is simple, the reaction temperature is room temperature, and the reaction does not require alcohol solvents, so the reaction is clean and efficient. Then, the phenolic resin-based carbon spheres with the same uniform particle size obtained after sintering and drying are fully ground with an activator, so that not only the activator and the phenolic resin-based carbon spheres can be fully combined, but also the phenolic resin-based carbon spheres can be further dispersed. Finally, the activator is sintered to remove the activator, and holes are formed on the surface of the phenolic resin-based carbon spheres, so that the finally prepared phenolic resin-based porous carbon spheres have dispersibility and a high specific surface area. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The present invention is a SEM image of a phenolic resin-based porous carbon sphere obtained by the preparation method of the present invention. DETAILED DESCRIPTION

[0030] Example 1

[0031] S1. Weigh 2,4-dihydroxybenzoic acid, triblock copolymer F127, ammonia water, formaldehyde, resorcinol and water in a mass ratio of 1:2:13:11:20:150 respectively; mix the weighed resorcinol and triblock copolymer F127 with water to prepare a mixed solution A; mix formaldehyde, 2,4-dihydroxybenzoic acid and ammonia water to prepare a mixed solution B;

[0032] S2, take 1 / 3 of the mixed solution B and add it dropwise to the mixed solution A at 25°C, mix and stir, and after the reaction is completed, add the remaining 2 / 3 of the mixed solution B dropwise to the mixed solution A in 4 batches to obtain a mixed solution C, the dropping rate is 50 drops / min, and the speed of the reactor is 230r / min;

[0033] S3, washing the mixed solution C with water, and drying it to obtain phenolic resin microspheres;

[0034] S4, heating the phenolic resin microspheres to 220° C. in a tube furnace and maintaining the temperature for 1 h, and then heating the temperature to 600° C. and maintaining the temperature for 1.5 h to obtain phenolic resin-based carbon spheres;

[0035] S5. Add 3 times the mass of sodium hydroxide to the phenolic resin-based carbon balls and grind for 0.8 hours. Then put them into a tubular furnace, heat them to 430°C and keep them for 0.8 hours, then heat them to 700°C and keep them for 1.5 hours. After taking them out of the furnace, wash them with water and dry them to obtain phenolic resin-based porous carbon balls.

[0036] Example 2

[0037] S1. Weigh salicylic acid, Tween 80, ammonia water, formaldehyde, m-aminophenol and water in a mass ratio of 1:1:6:3:10:100 respectively; mix the weighed m-aminophenol and Tween 80 with water to prepare a mixed solution A; mix formaldehyde, salicylic acid and ammonia water to prepare a mixed solution B;

[0038] S2, take 1 / 6 of the mixed solution B and add it dropwise to the mixed solution A, mix and stir at 15°C, and after the reaction is completed, add the remaining 5 / 6 of the mixed solution B dropwise to the mixed solution A in 5 batches to obtain a mixed solution C, with a dropwise acceleration rate of 40 drops / min and a reactor speed of 150r / min;

[0039] S3, washing the mixed solution C with water, and drying it to obtain phenolic resin microspheres;

[0040] S4, heating the phenolic resin microspheres to 180° C. in a tube furnace and maintaining the temperature for 0.5 h, and then heating the temperature to 400° C. and maintaining the temperature for 1 h to obtain phenolic resin-based carbon spheres;

[0041] S5. Add 2 times the mass of potassium hydroxide to the phenolic resin-based carbon spheres and grind for 0.5 h. Then put them into a tubular furnace, heat them to 400°C and keep them for 0.5 h, then heat them to 600°C and keep them for 1 h. After taking them out of the furnace, wash them with water and dry them to obtain phenolic resin-based porous carbon spheres.

[0042] Example 3

[0043] S1. Weigh sodium salicylate, OP-30, sodium carbonate, formaldehyde, p-aminophenol and water in a mass ratio of 1:3:20:18:30:200 respectively; mix the weighed p-aminophenol and OP-30 with water to prepare a mixed solution A; mix formaldehyde, sodium salicylate and sodium carbonate to prepare a mixed solution B;

[0044] S2, take 1 / 2 of the mixed solution B and add it dropwise to the mixed solution A at 35°C, mix and stir, and after the reaction is completed, add the remaining 1 / 2 of the mixed solution B dropwise to the mixed solution A in three batches to obtain a mixed solution C, with a dropwise acceleration rate of 60 drops / min and a reactor speed of 300r / min;

[0045] S3, washing the mixed solution C with water, and drying it to obtain phenolic resin microspheres;

[0046] S4, heating the phenolic resin microspheres to 250° C. in a tube furnace and maintaining the temperature for 1 h, and then heating the temperature to 800° C. and maintaining the temperature for 2 h to obtain phenolic resin-based carbon spheres;

[0047] S5. Add 4 times the mass of potassium hydroxide to the phenolic resin-based carbon balls and grind for 1 hour. Then put them into a tubular furnace, heat them to 450°C and keep them for 1 hour, then heat them to 800°C and keep them for 3 hours. After taking them out of the furnace, wash them with water and dry them to obtain phenolic resin-based porous carbon balls.

[0048] Comparative Example 1

[0049] Compared with Example 1, the difference is:

[0050] S2. Take 2 / 3 of the mixed solution B and add it dropwise to the mixed solution A, mix and stir at 25°C; after the reaction is completed, add the remaining 1 / 3 of the mixed solution B dropwise to the mixed solution A to obtain a mixed solution C. The dropping rate is 100 drops / min, and the speed of the reactor is 100 r / min.

[0051] The rest is the same as in Example 1.

[0052] Comparative Example 2

[0053] The difference from Example 1 is that:

[0054] S2. Take all the mixed solution B and add it dropwise to the mixed solution A, mix and stir at 25° C. to obtain a mixed solution C.

[0055] The rest is the same as in Example 1.

[0056] Comparative Example 3

[0057] The difference from Example 1 is that:

[0058] S5. Add 0.5 times the mass of sodium hydroxide to the phenolic resin-based carbon spheres and grind for 0.8 h. Then put them into a tubular furnace, first heat them to 430°C and keep them for 0.8 h, then heat them to 700°C and keep them for 1.5 h. After taking them out of the furnace, wash them with water and dry them to obtain phenolic resin-based porous carbon spheres.

[0059] The rest is the same as in Example 1.

[0060] Comparative Example 4

[0061] The difference from Example 1 is that:

[0062] S5. Add 5 times the mass of sodium hydroxide to the phenolic resin-based carbon balls and grind for 0.8h. Then put them into a tubular furnace, heat them to 430°C and keep them for 0.8h, then heat them to 700°C and keep them for 1.5h. After taking them out of the furnace, wash them with water and dry them to obtain phenolic resin-based porous carbon balls.

[0063] The rest is the same as in Example 1.

[0064] Test method:

[0065] 1. Use BET tester to test the specific surface area of ​​phenolic resin-based porous carbon spheres;

[0066] 2. Use a pore size distribution measuring instrument to measure the pore volume of phenolic resin-based porous carbon spheres;

[0067] 3. Use a pore size analyzer to measure the pore size of phenolic resin-based porous carbon spheres.

[0068] 4. Randomly select 50 phenolic resin-based porous carbon balls in each group, measure the particle size of each group of 50 phenolic resin-based porous carbon balls, and use the formula Calculate the standard deviation of particle size for each group;

[0069] Test Results

[0070] Group <![CDATA[Specific surface area / m 2 / g]]> <![CDATA[Pore volume / cm 3 / g]]> Pore ​​diameter / nm Particle size standard deviation / μm Example 1 1715 0.70 1.62 0.52 Example 2 1536 0.68 1.58 0.39 Example 3 2103 0.83 2.23 0.69 Comparative Example 1 1168 0.53 1.49 1.26 Comparative Example 2 965 0.38 0.73 3.36 Comparative Example 3 839 0.32 0.54 1.85 Comparative Example 4 1235 0.56 1.86 1.98

[0071] In Example 1-3, the proportion of each component and the mixing method of the mixed solution A / B are adjusted to prepare phenolic resin-based porous carbon spheres with high specific surface area and uniform particle size.

[0072] Compared with Example 1, Comparative Examples 1 and 2 changed the mixing mode of mixed solution A / B. Comparative Example 1 increased the drop rate and the speed of the reactor, and Comparative Example 2 added mixed solution B to mixed solution A at one time, resulting in a poor uniformity of the reaction, and thus the performance of the prepared phenolic resin-based porous carbon spheres decreased. Comparative Examples 3 and 4 changed the amount of activator added, resulting in changes in the holes of the phenolic resin-based porous carbon spheres, which directly affected their specific surface area. Too little activator dosage will reduce the number of holes on its surface, thereby reducing the specific surface area, and too much activator dosage will cause the collapse of the structure due to too many holes on its surface.

[0073] Although the present invention has been described in detail by reference to the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. A method for preparing phenolic resin-based porous carbon spheres, characterized in that: Follow the steps below to implement it: A phenol source, a dispersant and water are mixed to prepare a mixed solution A; formaldehyde, a stabilizer and a catalyst are mixed to prepare a mixed solution B; Divide the mixed solution B into at least two portions, and add one portion of the mixed solution B dropwise into the mixed solution A each time, and mix and stir at a high speed until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C; Drying the mixed solution C to obtain phenolic resin microspheres; sintering the phenolic resin microspheres to obtain phenolic resin-based carbon spheres; An activator is added to phenolic resin-based carbon spheres, and the phenolic resin-based porous carbon spheres are obtained by grinding and sintering.

2. The method for preparing phenolic resin-based porous carbon spheres according to claim 1, characterized in that: The step of dividing the mixed solution B into at least two portions, and adding one portion of the mixed solution B dropwise into the mixed solution A each time and mixing and stirring the mixture until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C also includes that each time the mixing is performed, the dropping speed of the mixed solution B is 40 to 60 drops / min, and the mixing and stirring temperature is 15° C. to 35° C.

3. The method for preparing phenolic resin-based porous carbon spheres according to claim 1 or 2, characterized in that: The step of dividing the mixed solution B into at least two portions and adding one portion of the mixed solution B dropwise into the mixed solution A for mixing and stirring each time further comprises dividing the mixed solution B into n portions, recording the mixed solution B added for the first time as B1, and recording the mixed solution B added for the second, third, ..., nth times as B2, B3, ..., Bn, respectively, wherein, by mass, B:B1=1:(1 / 6-1 / 2), and B2-Bn are equally divided.

4. The method for preparing phenolic resin-based porous carbon spheres according to any one of claims 1 to 3, characterized in that: The high-speed mixing and stirring is performed using a reactor, and the rotation speed of the reactor is 150-300 rad / min.

5. The method for preparing phenolic resin-based porous carbon spheres according to claim 1, characterized in that: The mass ratio of the phenol source, dispersant, water, formaldehyde, catalyst and stabilizer is (10-30):(1-3):(100-200):(3-18):(6-20):

1.

6. The method for preparing phenolic resin-based porous carbon spheres according to claim 1, characterized in that: The phenol source is selected from one or more of p-aminophenol, m-aminophenol, o-aminophenol, resorcinol, catechol, hydroquinone, and phloroglucinol; the activator is selected from one or more of sodium hydroxide, potassium hydroxide, calcium chloride, and zinc chloride.

7. The method for preparing phenolic resin-based porous carbon spheres according to claim 1, characterized in that: The dispersant is selected from one or more of Tween 80, Tween 60, polyvinyl alcohol, polypyrrolidone, polyethylene glycol, sodium dodecyl sulfonate, sodium dodecyl sulfate, hexadecyl ammonium bromide, OP-30, and triblock copolymer F127; the stabilizer is selected from one or more of salicylic acid, sodium salicylate, 4-amino-2-hydroxybenzoic acid, phloroglucinol formic acid, 2,4-dihydroxybenzoic acid, and 3,5-dihydroxybenzoic acid; the catalyst is selected from one or more of ammonia water, triethylamine, sodium hydroxide, potassium hydroxide, barium hydroxide, magnesium hydroxide, and sodium carbonate.

8. The method for preparing phenolic resin-based porous carbon spheres according to claim 1, characterized in that: The sintering of the phenolic resin microspheres to obtain the phenolic resin-based carbon spheres includes the following sintering process: firstly heating to 180-250° C. and maintaining for 0.5-1 hour, and then heating to 400-800° C. and maintaining for 1-2 hours.

9. The method for preparing phenolic resin-based porous carbon spheres according to claim 1, characterized in that: The amount of the activator is 2 to 4 times the mass of the phenolic resin-based carbon spheres; The method of adding an activator to the phenolic resin-based carbon spheres, grinding, and sintering to obtain the resin-based porous carbon spheres comprises: The grinding time after adding the activator to the phenolic resin-based carbon spheres is 0.5 to 1 h; The sintering process is to first heat the temperature to 400-450°C and keep it for 0.5-1h, then heat it to 600-800°C and keep it for 1-3h, and finally cool it to room temperature with the furnace.

10. A phenolic resin-based porous carbon sphere, characterized in that: The phenolic resin-based porous carbon spheres are prepared by the preparation method of any one of claims 1 to 9.