Porous carbon material with high tetracycline adsorption capacity and preparation method thereof

Porous carbon particles were prepared by co-activated NaOH-Na2CO3 on industrial coconut shell activated carbon, which solved the problems of low adsorption capacity of existing adsorption materials on tetracycline and difficult separation of materials, and achieved efficient and low-cost tetracycline removal effect.

CN118908211APending Publication Date: 2024-11-08GUANGZHOU UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411077676.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing adsorption materials have low adsorption capacity to tetracycline, and the fine powdered materials are difficult to separate and recover in water bodies, which is high in preparation costs, which affects the efficient removal of tetracycline pollutants in water bodies.

Method used

Low-priced industrial coconut shell activated carbon was used to co-activate NaOH-Na2CO3 to prepare porous carbon particles with high specific surface area and developed pore structure for efficient adsorption and removal of tetracycline.

Benefits of technology

It has achieved high tetracycline adsorption capacity and efficient removal rate, uniform particle shape, simple operation, low production cost, and good industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908211A_ABST
    Figure CN118908211A_ABST
Patent Text Reader

Abstract

The invention discloses a porous carbon material with high tetracycline adsorption capacity and a preparation method thereof, and belongs to the technical field of wastewater adsorption treatment material preparation, and the preparation method comprises the following steps: (1) preparing coconut shell charcoal; (2) adding the coconut shell charcoal into a mixed solution of sodium hydroxide and sodium carbonate for dipping, and drying to obtain loaded coconut shell charcoal; and (3) placing the loaded coconut shell charcoal in nitrogen flow for high-temperature activation, and then sequentially washing and drying to obtain the coconut shell charcoal. The porous carbon particle material disclosed by the invention is uniform in particle morphology, has high adsorption capacity and adsorption removal efficiency on TC, and has a good industrial application prospect in the aspect of efficiently adsorbing and removing TC.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater adsorption treatment material preparation, and in particular to a porous carbon material with high tetracycline adsorption capacity and a preparation method thereof. Background Art

[0002] Tetracycline (TC) is a commonly used veterinary antibiotic that can prevent and treat various diseases of livestock, promote livestock growth, and improve livestock physical fitness. However, TC ingested by livestock will not be completely absorbed in the animal body, and will enter the water and soil with the animal's excrement, polluting the ecological environment; at the same time, TC has a high solubility in water, a long half-life, and a stable structure. It can enter the human body through the food chain, posing a great threat to human health. Therefore, it is urgent to efficiently remove TC from water.

[0003] At present, the TC removal technologies that have been studied more include microbial degradation technology (Li Y, Zhang G, Liang D, et al. Tetracycline hydrochloride degradation in polarity inverted microbial fuel cells: Performance, mechanisms and microbiology [J] Chemosphere, 2024, 349, 140902), chlorination technology (Sompornpailin D, Pulgerd P, Sangsanont J, et al. Removal of antibiotics, bacterial toxicity, and occurrence of antibiotic resistance genes in secondary hospital effluents treated with granular activated carbon and the impact of preceding chlorination [J] Science of The Total Environment, 2024, 927, 172095), and advanced oxidation technology (Amangelsin Y, Semenova Y, Dadar M, et al. The Impact of TetracyclinePollution on the Aquatic Environment and Removal Strategies[J]Antibiotics,2023,12(3),440), electrochemical treatment technology(Dai Y,Liu M,Li J,et al.A review on pollution situation and treatment methods of tetracycline in groundwater[J]Separation Science and Technology,2019,55(5),1005), adsorption technology(Yan L,Song X,Miao J,etal.Removal of tetracycline from water by adsorption with biochar:Areview[J]Journal of Water Process Engineering,2024,60,105215), membrane separation technology (Guo R, Qin W, Wang B, etal.NH2-MIL-88B(Fe) / TiO2 / PAN electrostatically spun nanofiber membrane for photocatalytic degradation of tetracycline and oil-water separation[J]Separation and Purification Technology, 2024, 351, 128059) and ultrasonic cavitation effect technology (HouL, Zhang H, Xue Compared with other treatment technologies, adsorption technology is the most promising TC removal technology for industrial application due to its advantages of low cost, simple operation, high removal efficiency, and no production of highly toxic byproducts.

[0004] The efficiency of the adsorption process is affected by the properties of the adsorbent material and the adsorbate, among which the specific surface area, porosity, pore size and surface chemical properties of the adsorbent material greatly affect the adsorption efficiency. Traditional adsorption materials such as activated carbon (JiL, Chen W, Duan L, et al. Mechanisms for strong adsorption of tetracycline to carbon nanotubes: A comparative study using activated carbon and graphite as adsorbents [J] Environmental Science & Technology, 2009, 43 (7), 2322), clay and minerals (Gao J, Pedersen J. Adsorption of Sulfonamide Antimicrobial Agents to Clay Minerals [J] Environmental Science & Technology, 2005, 39 (24), 9509), zeolite composites (Al-Salihi S, Fidalgo M, Xing Y. Fast Removal of Tetracycline from Aqueous Solution by Aluminosilicate Zeolite Nanoparticles with High Adsorption Capacity [J] ACS EST Water, 2023, 3 (3), 838), metals and their oxides (Hsu L, Liu Y, Syu C,etal.Adsorption of tetracycline on Fe(hydr)oxides:effects of pH and metalcation(Cu 2+ ,Zn 2+ and Al 3+)addition in various molar ratios[J]Royal Society OpenScience,2018,5,171941) Due to its low specific surface area, underdeveloped pore structure, and relatively single functional groups, its adsorption capacity for TC is low. Therefore, the research and development of adsorption materials with large specific surface area, developed pore structure, and stable structure is the focus of developing efficient adsorption and removal of TC. New carbon-based porous materials have the characteristics of high specific surface area, rich pores, high water stability and acid-base stability (Wang Y,Xu L,Wei F,et al.Insights into the adsorption mechanism of tetracycline on hierarchically porous carbon and the effect ofnanoporous geometry[J]Chemical Engineering Journal,2022,437,135454), and are potential materials for adsorbing and removing TC from water pollutants. In addition, most of the new porous adsorption materials currently developed are in the form of fine powders. If they are directly used for the adsorption and removal of TC in water, they will face the problems of secondary pollution of the water and difficulty in separating and recovering the adsorption materials from the water. Generally, the fine powder materials must be reprocessed / molded before they can be used in practice, and the preparation cost is relatively high. Therefore, the development of molded carbon-based adsorption materials with high TC adsorption capacity is a subject of great practical value and economic benefits.

[0005] In order to prepare a shaped carbon-based adsorption material with high TC adsorption capacity and stable structure, this project invented a method of using low-cost industrial coconut shell activated carbon as raw material, co-activating it with NaOH-Na2CO3, and preparing porous carbon particles with high specific surface area and developed pore structure. This material has high TC adsorption capacity, excellent TC adsorption and removal efficiency, and uniform particle morphology, and has good industrial application prospects in the efficient adsorption and removal of TC. Summary of the invention

[0006] In view of the above problems, the present invention provides a porous carbon material with high tetracycline adsorption capacity and a preparation method thereof. The material adopts inexpensive industrial coconut shell activated carbon as a raw material, and co-activates the carbon with NaOH-Na2CO3 to prepare porous carbon particles with high specific surface area and developed pore structure. The porous carbon particles have high TC adsorption capacity and adsorption removal efficiency, and the particle morphology is uniform, and the material has good industrial application prospects in the efficient adsorption and removal of TC.

[0007] The purpose of the present invention is achieved by adopting the following technical solutions:

[0008] A method for preparing a porous carbon material with high tetracycline adsorption capacity comprises the following steps:

[0009] (1) preparing coconut shell charcoal;

[0010] (2) adding the coconut shell charcoal into a mixed solution of sodium hydroxide and sodium carbonate for immersion, and drying to obtain the loaded coconut shell charcoal;

[0011] (3) placing the loaded coconut shell charcoal in a nitrogen stream for high temperature activation, and then washing and drying in sequence to obtain the charcoal.

[0012] In some preferred embodiments, the method for preparing coconut shell charcoal comprises the following steps:

[0013] The coconut shell activated carbon is dry-ground, particles with a particle size between 35 mesh and 50 mesh are screened, and the coconut shell charcoal is obtained after washing and drying.

[0014] In some preferred embodiments, the concentration ratio of the sodium hydroxide to the sodium carbonate in the mixed solution in step (2) is 1:(1-4).

[0015] In some preferred embodiments, the concentration of sodium hydroxide in the mixed solution in step (2) is 0.02-0.25 mol / L, and the concentration of sodium carbonate is 0.08-0.4 mol / L.

[0016] In some preferred embodiments, the immersion time in step (2) is 6-12 hours.

[0017] In some preferred embodiments, the temperature of the high temperature activation in step (3) is 700-900° C., and the high temperature activation time is 60-120 min.

[0018] In some preferred embodiments, the heating rate of the high temperature activation is 1-5°C / min.

[0019] Another aspect of the present invention is to provide a porous carbon material with high tetracycline adsorption capacity, wherein the porous carbon material is prepared by the aforementioned preparation method.

[0020] The beneficial effects of the present invention are:

[0021] (1) The porous carbon particles of the present invention have uniform particle morphology, high TC adsorption capacity and adsorption removal efficiency. The porous carbon particles have an adsorption capacity of TC of 1244 mg / g (at 25°C); within 120 minutes after the adsorption begins, the removal rate of TC by the porous carbon particles is as high as 0.96 (at 25°C, the initial concentration of TC is 200 mg / L), which has a good industrial application prospect in the efficient adsorption removal of TC.

[0022] (2) The raw materials used in the present invention are industrial coconut shell activated carbon, NaOH and Na2CO3, which are widely available, inexpensive and have low production costs.

[0023] (3) The preparation method of the present invention mainly includes impregnation and high-temperature activation, which is simple to operate, easy to implement and has good repeatability. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0025] Figure 1 is the saturated adsorption capacity of porous carbon particles 1#-5# for TC;

[0026] Figure 2 is the adsorption kinetic curve of TC by porous carbon particles 1#-5#;

[0027] Figure 3 is the removal rate of TC in water by porous carbon particles 1#-5#;

[0028] Figure 4 It is the removal rate of TC in water by porous carbon particles 5# at different pH values. DETAILED DESCRIPTION

[0029] The present invention is further described in conjunction with the following examples.

[0030] Example 1

[0031] A porous carbon particle with high tetracycline adsorption capacity, the preparation method of which comprises the following steps:

[0032] (1) Weighing 5.0 g of industrial coconut shell activated carbon in block form and dry-grinding it, screening the dry-grinded coconut shell activated carbon with 50-mesh and 35-mesh sieves to obtain coconut shell carbon particles with a size ranging from 0.3 to 0.5 mm; washing the coconut shell carbon particles with 500 mL of deionized water for 3 times, and drying them in a forced air drying oven at 100° C. for 12 h to obtain coconut shell carbon particles with uniform particle size;

[0033] (2) Weigh 0.40 g of NaOH and 4.24 g of Na2CO3 respectively and dissolve them in 500 mL of water to obtain a NaOH-Na2CO3 mixed solution, wherein the concentration of NaOH is 0.02 mol / L and the concentration of Na2CO3 is 0.08 mol / L; take 1.0 g of the coconut shell charcoal particles obtained in step (1) and immerse them in the above-prepared NaOH-Na2CO3 mixed solution for 6 h, filter, and dry them in a 100° C. forced air drying oven for 12 h to obtain NaOH-Na2CO3-loaded coconut shell charcoal particles;

[0034] (3) The coconut shell charcoal particles obtained in step (2) were loaded into a porcelain boat, placed in a tubular furnace, and heated to 700°C at a heating rate of 1°C / min in a flowing nitrogen atmosphere (20 mL / min), and maintained for 60 min for high-temperature activation; after the activation was completed, the product was cooled to room temperature, washed with deionized water until the filtrate was neutral, and placed in a 100°C forced air drying oven for 12 h to obtain the porous carbon particles, which were recorded as material 1#.

[0035] Example 2

[0036] A porous carbon particle with high tetracycline adsorption capacity, the preparation method of which comprises the following steps:

[0037] (1) Same as Example 1;

[0038] (2) Weigh 1.00 g of NaOH and 2.65 g of Na2CO3 respectively and dissolve them in 500 mL of water to obtain a NaOH-Na2CO3 mixed solution, wherein the concentration of NaOH is 0.05 mol / L and the concentration of Na2CO3 is 0.05 mol / L; take 1.0 g of the coconut shell charcoal particles obtained in step (1) and immerse them in the above-prepared NaOH-Na2CO3 mixed solution for 6 h, filter, and dry them in a 100° C. forced air drying oven for 12 h to obtain NaOH-Na2CO3-loaded coconut shell charcoal particles;

[0039] (3) The coconut shell charcoal particles obtained in step (2) were loaded into a porcelain boat, placed in a tubular furnace, and heated to 700°C at a heating rate of 1°C / min in a flowing nitrogen atmosphere (20 mL / min), and maintained for 60 min for high-temperature activation; after the activation was completed, the product was cooled to room temperature, washed with deionized water until the filtrate was neutral, and placed in a 100°C forced air drying oven for 12 h to obtain the porous carbon particles, which were recorded as material 2#.

[0040] Example 3

[0041] A porous carbon particle with high tetracycline adsorption capacity, the preparation method of which comprises the following steps:

[0042] (1) Same as Example 1;

[0043] (2) Weigh 2.00 g of NaOH and 10.60 g of Na2CO3 respectively and dissolve them in 500 mL of water to obtain a NaOH-Na2CO3 mixed solution, wherein the concentration of NaOH is 0.10 mol / L and the concentration of Na2CO3 is 0.20 mol / L; take 1.0 g of the coconut shell charcoal particles obtained in step (1) and immerse them in the above-prepared NaOH-Na2CO3 mixed solution for 9 h, filter, and dry them in a 100° C. forced air drying oven for 12 h to obtain NaOH-Na2CO3-loaded coconut shell charcoal particles;

[0044] (3) The coconut shell charcoal particles obtained in step (2) were loaded into a porcelain boat, placed in a tubular furnace, and heated to 800°C at a heating rate of 3°C / min in a flowing nitrogen atmosphere (20 mL / min), and maintained for 100 min for high-temperature activation; after the activation was completed, the product was cooled to room temperature, washed with deionized water until the filtrate was neutral, and placed in a 100°C forced air drying oven for 12 h to obtain the porous carbon particles, which were recorded as material 3#.

[0045] Example 4

[0046] A porous carbon particle with high tetracycline adsorption capacity, the preparation method of which comprises the following steps:

[0047] (1) Same as Example 1;

[0048] (2) Weigh 2.00 g of NaOH and 21.20 g of Na2CO3 respectively and dissolve them in 500 mL of water to obtain a NaOH-Na2CO3 mixed solution, wherein the concentration of NaOH is 0.10 mol / L and the concentration of Na2CO3 is 0.40 mol / L; take 1.0 g of the coconut shell charcoal particles obtained in step (1) and immerse them in the above-prepared NaOH-Na2CO3 mixed solution for 12 h, filter, and dry them in a 100° C. forced air drying oven for 12 h to obtain NaOH-Na2CO3-loaded coconut shell charcoal particles;

[0049] (3) The coconut shell charcoal particles obtained in step (2) were loaded into a porcelain boat, placed in a tubular furnace, and heated to 900°C at a heating rate of 5°C / min in a flowing nitrogen atmosphere (20 mL / min), and maintained for 120 min for high-temperature activation; after the activation was completed, the product was cooled to room temperature, washed with deionized water until the filtrate was neutral, and placed in a 100°C forced air drying oven for 12 h to obtain the porous carbon particles, which were recorded as material 4#.

[0050] Example 5

[0051] A porous carbon particle with high tetracycline adsorption capacity, the preparation method of which comprises the following steps:

[0052] (1) Same as Example 1;

[0053] (2) Weigh 5.00 g of NaOH and 13.25 g of Na2CO3 respectively and dissolve them in 500 mL of water to obtain a NaOH-Na2CO3 mixed solution, wherein the concentration of NaOH is 0.25 mol / L and the concentration of Na2CO3 is 0.25 mol / L; take 1.0 g of the coconut shell charcoal particles obtained in step (1) and immerse them in the above-prepared NaOH-Na2CO3 mixed solution for 12 h, filter, and dry them in a 100° C. forced air drying oven for 12 h to obtain NaOH-Na2CO3-loaded coconut shell charcoal particles;

[0054] (3) The coconut shell charcoal particles obtained in step (2) were loaded into a porcelain boat, placed in a tubular furnace, and heated to 900°C at a heating rate of 5°C / min in a flowing nitrogen atmosphere (20 mL / min), and maintained for 120 min for high-temperature activation; after the activation was completed, the product was cooled to room temperature, washed with deionized water until the filtrate was neutral, and placed in a 100°C forced air drying oven for 12 h to obtain the porous carbon particles, which were recorded as material 5#.

[0055] The control example is a block of industrial coconut shell activated carbon without any treatment, which is recorded as material 0#.

[0056] Experimental example

[0057] The porous carbon particles 0# of the control example and 1#-5# prepared in each of Examples 1-5 were subjected to pore structure characterization and TC adsorption performance testing to evaluate the adsorption and removal capacity of the porous carbon particles for TC in water.

[0058] The pore structure parameters were obtained by testing the nitrogen adsorption-desorption curve at -196℃ on the Micromeritics ASAP 2460 multi-station extended automatic specific surface area and porosity analyzer. In the saturated adsorption capacity determination experiment, 10 mg of porous carbon particles were placed in 50 mL of TC solution with an initial concentration of 200 mg / L and stirred in a dark box; after stirring for 24 hours, the solution was taken out and filtered, and the concentration of tetracycline in the filtrate was determined by high performance liquid chromatography (Agilent 1260Infinity II), and then the adsorption capacity of porous carbon particles for TC was calculated, which was recorded as the saturated adsorption capacity. In the adsorption kinetics experiment, 10 mg of porous carbon particles were placed in 50 mL of TC solution with an initial concentration of 200 mg / L and stirred in a dark box; after stirring for a certain period of time, the solution was taken out and filtered, and the concentration of tetracycline in the filtrate was determined by high performance liquid chromatography (Agilent 1260Infinity II), and then the adsorption capacity of porous carbon particles for TC and the removal rate of TC in water were calculated.

[0059] The present invention also conducts a pH influence test on the better samples, using HCl and NaOH solutions to adjust the pH value of the TC solution with an initial concentration of 200 mg / L, the initial pH of the solution = 2.0-10.3, then 10 mg of porous carbon particles are placed in TC solutions with different pH values, and placed in a dark box for stirring; after stirring for 120 minutes, the solution is taken out and filtered, and the concentration of tetracycline in the filtrate is determined by high performance liquid chromatography (Agilent 1260Infinity II), and then the removal rate of TC in water by the porous carbon particles is calculated.

[0060] The above TC adsorption experiments were all carried out at 25 °C.

[0061] The calculation formulas for the adsorption capacity of porous carbon particles for TC and the removal rate of TC in water are shown in equations (1) and (2), respectively.

[0062]

[0063]

[0064] In the formula, Q t (mg / g) represents the adsorption capacity at time t; C0 and C t (mg / L) are the initial concentration of TC in the solution and the concentration at time t, respectively; V and m are the volume of solution (50 mL) and the mass of porous carbon particles (10 mg) used in the adsorption process, respectively; ρ is the removal rate of TC by porous carbon particles.

[0065] The characterization and test results are as follows:

[0066] (1) Pore structure parameters of porous carbon particles 1#-5#

[0067] Compared with the control example 0#, the porous carbon particles 1#-5# prepared in Examples 1 to 5 have high specific surface areas and developed pore structures. The specific surface areas and total pore volume parameters are shown in Table 1. Among them, the BET specific surface area of ​​the porous carbon particles 5# prepared in Example 5 is the largest, reaching 2620 m 2 / g, the total pore volume reaches 1.48cm 3 / g; with the increase of NaOH-Na2CO3 mixed solution concentration, activation temperature and activation time, the specific surface area and pore volume of the prepared porous carbon particles continue to increase, which shows that the activator, activation temperature and activation time have a great influence on the pore structure of the porous carbon particles.

[0068] Table 1 Pore structure parameters of porous carbon particles 1#-5#

[0069] sample <![CDATA[S BET (m 2 / g)]]> <![CDATA[V total (cm 3 / g)]]> 0# 10.2 0.008 1# 1337 0.56 2# 1545 0.70 3# 2192 0.88 4# 2476 1.19 5# 2620 1.48

[0070] (2) Adsorption performance of porous carbon particles 1#-5# on TC

[0071] The saturated adsorption capacity of porous carbon particles 1-5# prepared in Examples 1-5 and 0# in the control example for TC is shown in the attached Figure 1 .from Figure 1 It can be seen that compared with the reference example 0#, the porous carbon particles prepared in the embodiment of the present invention have greatly improved the saturated adsorption capacity of TC at 25°C, which is as high as 1244 mg / g. The adsorption capacity of porous carbon particles for TC is closely related to the pore structure parameters of the material. The material with large specific surface area and pore volume has high saturated adsorption capacity for TC.

[0072] The adsorption kinetics curve of TC by porous carbon particles 1-5# prepared in Example 1-5 is shown in the attached Figure 2 .from Figure 2 It can be seen that within the first 20 minutes of adsorption, the adsorption capacity of TC by the porous carbon particles prepared in each embodiment increases rapidly. This is because in the initial stage of adsorption, the mass transfer driving force brought by the high concentration gradient between the porous carbon particles and the TC solution interface is conducive to rapid adsorption.

[0073] The removal rate of TC in water by porous carbon particles 1-5# prepared in Example 1-5 is shown in the attached Figure 3 .from Figure 3 It can be seen that within 120 minutes after the adsorption, the adsorption removal rate of TC by porous carbon particles is as high as 0.96, which has the potential to efficiently adsorb and remove TC from water.

[0074] (3) Acid-base stability of porous carbon particles 5#

[0075] The removal rate of TC in water by porous carbon particles 5# prepared in Example 5 at different pH values ​​is shown in the attached Figure 4 .from Figure 4 It can be seen that in the original TC solution (without pH adjustment, pH = 5.0), within 120 minutes after the adsorption, the adsorption removal rate of TC by porous carbon particles was as high as 0.96; after adding acid / base to adjust the initial pH value of the solution, the adsorption removal rate of TC by porous carbon particles decreased within the same period of time, but still remained above 0.80, indicating that the adsorption and removal performance of TC in water by porous carbon particles has good acid-base stability.

[0076] According to the above results of this experimental example, it can be seen that the porous carbon particle material prepared by the present invention has uniform particle morphology, developed pore structure, high TC adsorption capacity and adsorption removal efficiency, and has good application prospects in the efficient adsorption and removal of TC pollutants in water bodies.

[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a porous carbon material with high tetracycline adsorption capacity, characterized in that: The following steps are involved: (1) preparing coconut shell charcoal; (2) adding the coconut shell charcoal into a mixed solution of sodium hydroxide and sodium carbonate for immersion, and drying to obtain the loaded coconut shell charcoal; (3) placing the loaded coconut shell charcoal in a nitrogen stream for high temperature activation, and then washing and drying in sequence to obtain the charcoal.

2. The method for preparing a porous carbon material with high tetracycline adsorption capacity according to claim 1, characterized in that: The preparation method of coconut shell charcoal comprises the following steps: The coconut shell activated carbon is dry-ground, particles with a particle size between 35 mesh and 50 mesh are screened, and the coconut shell charcoal is obtained after washing and drying.

3. The method for preparing a porous carbon material with high tetracycline adsorption capacity according to claim 1, characterized in that: The concentration ratio of the sodium hydroxide to the sodium carbonate in the mixed solution in step (2) is 1:(1-4).

4. The method for preparing a porous carbon material with high tetracycline adsorption capacity according to claim 1, characterized in that: The concentration of the sodium hydroxide in the mixed solution in step (2) is 0.02-0.25 mol / L, and the concentration of the sodium carbonate is 0.08-0.4 mol / L.

5. The method for preparing a porous carbon material with high tetracycline adsorption capacity according to claim 1, characterized in that: The immersion time in step (2) is 6-12 hours.

6. The method for preparing a porous carbon material with high tetracycline adsorption capacity according to claim 1, characterized in that: The temperature of the high temperature activation in step (3) is 700-900° C., and the high temperature activation time is 60-120 min.

7. The method for preparing a porous carbon material with high tetracycline adsorption capacity according to claim 6, characterized in that: The heating rate of the high temperature activation is 1-5°C / min.

8. A porous carbon material with high tetracycline adsorption capacity, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation of coir fiber based activated carbon with high specific surface area

    CN101428794A

  • Preparation method of high-penetration microporous granular active carbon

    CN106006638A

  • Camphor tree-base porous activated carbon, preparation method thereof and application of camphor tree-base porous activated carbon in electrochemical energy storage

    CN108715447A

  • Method for adsorbing aureomycin antibiotic by using modified coconut shell charcoal

    CN114789041A

  • Water treatment catalyst as well as preparation method and application thereof

    CN117299127A