Nanometer flaky rare earth oxide and preparation method thereof

Controlling the preparation of rare earth oxides by liquid phase co-precipitation method, the problems of expensive equipment, low yield and difficult to control morphological uniformity in the prior art are solved, and low-cost, simple and easy-to-operate nanosheet rare earth oxides are realized The industrial production has obtained nano- and micro-nano-scale products with uniform morphology and high dispersion.

CN118908264APending Publication Date: 2024-11-08BAOTOU RESEARCH INSTITUTE OF RARE EARTHS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410950928.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing preparation methods for nanosheet-shaped rare earth oxides have problems such as expensive equipment, low yield, environmental pollution, high cost, complex process and difficult to control, especially the liquid phase method has challenges in morphological uniformity and industrial production.

Method used

By controlling the relative drop rate and alkalinity selection of rare earth solution and mixed precipitant, the crystal growth direction is regulated, and combined with the control of reaction temperature, the 30-100nm nanoscale and 100-300nm micro-nanoscale are prepared. Nanoflake rare earth oxides achieve low-cost, simple and easy-to-operate industrial production.

Benefits of technology

The morphological uniformity of nano- and micro-nano-scale rare earth oxides is achieved, the preparation cost is reduced, the process flow is simplified, centrifugal operations are avoided, suitable for industrial production, and dispersion is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908264A_ABST
    Figure CN118908264A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nano materials, in particular to a nano flaky rare earth oxide and a preparation method thereof. According to the specific technical scheme, the preparation method of the nanosheet-shaped rare earth oxide comprises the following steps: dropwise adding a rare earth solution and excessive carbonized ammonia water precipitant into a base solution at the same time, carrying out a heat preservation reaction, and after the reaction is finished, calcining a precursor to obtain the nanosheet-shaped rare earth oxide. The preparation cost is low, equipment is simple and easy to operate, the prepared nanosheet-shaped rare earth oxide precursor is easy to filter, centrifugal operation is not needed, and industrial production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano materials, and in particular to a nano sheet-like rare earth oxide and a preparation method thereof. Background Art

[0002] Nanomaterials have many excellent properties, such as quantum size effect, small size effect, surface and interface effect, and macroscopic quantum tunneling effect. These excellent properties make them a hot topic in current research. Nano rare earth materials have the properties of both nano materials and rare earth compounds. They have excellent properties due to their special morphology. Among them, two-dimensional nano rare earth compounds have attracted attention due to their high specific surface area, high anisotropy, and ultra-thin thickness. They are widely used in luminescence, fluorescent probes, catalysis, storage devices, and batteries, greatly improving the performance of materials.

[0003] Nano-sheet rare earth oxides can be prepared by three methods: gas phase method, solid phase method and liquid phase method. The solid phase synthesis process has the disadvantages of large particle size and uneven dispersion, and the gas phase synthesis process has the disadvantages of expensive equipment, low yield and unsuitability for industrialization. The liquid phase method can overcome these disadvantages and has therefore become a research hotspot in recent years. Liquid phase synthesis methods include microemulsion method, sol-gel method, spray pyrolysis method, liquid phase precipitation method, etc. In the literature Ceramics International 41 (2015) 3999-4006, a dysprosium hydroxide precursor was successfully prepared by hydrothermal method, and Dy2O3 with nanosheet and nanorod morphology was obtained after high temperature treatment. J Phys Chem 2009, 113, 50, 21034-21041 reported a method of dissolving Dy(acac)3 in benzyl alcohol, heating it to 200°C, and then calcining the resulting product at 500°C to obtain layered Dy2O3 nanosheet microspheres by a non-aqueous sol-gel method. J Nanopart Res (2013) 15: 1944 successfully synthesized 60-80nm CeO2 sheets by benzyl alcohol-assisted solvothermal reaction. Journal of Solid State Chemistry 290 (2020) 121593 synthesized Ce2CO3.6H2O nanosheets with uniform morphology and a thickness of about 180nm by carbonization of carbon dioxide. However, the above methods have the disadvantages of environmental pollution, high cost, complex process, difficulty in control and difficulty in industrialization. In the liquid phase precipitation method, a mixed precipitant is often used to precipitate a rare earth solution to prepare rare earth oxides and their precursors. Rare Metals and Cemented Carbides. 2017, 45(02) used ammonium bicarbonate and ammonia water as a mixed precipitant with a molar ratio of 1:1.04 to precipitate lanthanum chloride, and obtained a mixture of spherical lanthanum carbonate and lanthanum basic carbonate. Journal of the Chinese Society of Rare Earths ISSN 1000-4343, CN11-2365 / TG used a co-current liquid phase precipitation method to precipitate lanthanum chloride with a mixed precipitant of ammonium bicarbonate and ammonia water to prepare a flower-like lanthanum carbonate. It can be seen that if you want to obtain nano-sheet rare earth compounds by liquid phase precipitation, you need to accurately control the reaction conditions and understand the key factors that affect the morphology of the compound during the precipitation process. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a nano-flaky rare earth oxide and a preparation method thereof, which adopts a liquid phase coprecipitation method, and regulates the crystal growth direction by controlling the relative dripping speed of the rare earth solution and the mixed precipitant and selecting the alkalinity of the mixed precipitant, and regulates the thickness of the rare earth oxide sheet by changing the reaction temperature, thereby obtaining 30-100nm nano-scale and 100-300nm micro-nano-scale flaky rare earth oxide with good dispersibility. The method is low in cost, simple and easy to operate, and can realize industrial production.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0006] The invention discloses a method for preparing nano-flaky rare earth oxides. Rare earth solution and excess carbonized ammonia water precipitant are simultaneously added dropwise to a base liquid for heat preservation reaction. After the reaction is completed, the precursor is calcined to obtain the nano-flaky rare earth oxides.

[0007] Preferably, the mass volume concentration of the rare earth solution is 10 to 320 g / L; 2- The molar concentration of the carbonized ammonia water precipitant is 1.5-2.3 mol / L.

[0008] Preferably, the NH3:CO3 in the carbonized ammonia precipitation agent 2- The molar ratio is 1:1.5~3.5.

[0009] Preferably, the RE of the rare earth solution and the carbonized ammonia precipitant solution is 3+ :CO3 2- The molar ratio is 1:2.0~3.5.

[0010] Preferably, the relative dripping rate ratio of the rare earth solution and the carbonized ammonia water precipitant is 1:1.5-2.0.

[0011] Preferably, the rare earth solution is one or more of rare earth nitrate, rare earth chloride, rare earth sulfate, and rare earth acetate.

[0012] Preferably, the temperature of the insulation reaction is 0-90° C., the time is 0.5-1 h, and the calcination temperature is 700-900° C., and the time is 1-4 h.

[0013] Preferably, when the reaction temperature is 0-60°C, the thickness of the prepared rare earth oxide flakes is 30-100 nm; when the reaction temperature is 60-90°C, the thickness of the prepared rare earth oxide flakes is 100-300 nm.

[0014] Preferably, after the reaction is completed, the pH value of the reaction solution is ≥8.

[0015] Correspondingly, the nano-flaky rare earth oxide prepared by the above preparation method has a sheet thickness of 30 to 300 nm.

[0016] The present invention has the following beneficial effects:

[0017] 1. Compared with the hydrothermal method and sol-gel method used to prepare nano rare earth oxides, the liquid phase precipitation method used in the present invention has low cost, simple equipment and easy operation. The prepared nano rare earth oxide precursor is easy to filter and does not require centrifugation operation, so it can be industrialized.

[0018] 2. The present invention controls the relative dripping rate of the rare earth solution and the excess carbonized ammonia precipitant and selects the alkalinity of the precipitant to adjust the crystal growth direction to obtain nano-flaky rare earth oxides. The thickness of the nano-rare earth oxide flakes is adjusted by changing the reaction temperature to finally obtain nano-scale and micro-nano-scale flaky rare earth oxides with uniform morphology and a flake thickness of 30 to 100 nm and 100 to 300 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The present invention is a flow chart for preparing the nano-sheet rare earth oxide;

[0020] Figure 2 This is a SEM image of the nano-sheet lanthanum oxide prepared in Example 1;

[0021] Figure 3 This is a SEM image of lanthanum oxide prepared in Comparative Example 1;

[0022] Figure 4 This is a SEM image of lanthanum oxide prepared in Comparative Example 2;

[0023] Figure 5 This is the SEM image of lanthanum oxide prepared in Comparative Example 3. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0026] 1.Reference Figure 1 As shown, the present invention discloses a method for preparing nano-sheet rare earth oxides, and the process is as follows:

[0027] The rare earth solution and an excess of carbonized ammonia water precipitant are simultaneously added dropwise to the bottom liquid for heat preservation reaction. After the reaction is completed, the reaction liquid is filtered, the precursor is washed, dried, and calcined to obtain nano-sheet rare earth oxides.

[0028] The rare earth solution is one or more of rare earth nitrate, rare earth chloride, rare earth sulfate and rare earth acetate, and has a mass volume concentration of 10 to 320 g / L, more preferably 10 to 100 g / L.

[0029] The carbonized ammonia precipitation agent, NH3:CO3 2- The molar ratio is 1:1.5~3.5; CO3 2- The molar concentration is 1.5 to 2.3 mol / L, more preferably 1.8 to 2.2 mol / L.

[0030] The rare earth solution and the excess carbonized ammonia precipitant solution are added dropwise at the same time. 3+ :CO3 2- The molar ratio is 1:2.0-3.5; the relative dripping rate ratio of the rare earth solution and the carbonized ammonia precipitant is 1:1.5-2.0. The liquid phase co-precipitation method is adopted to adjust the crystal growth direction by selecting the alkalinity of the carbonized ammonia precipitant and controlling the relative dripping rate of the rare earth solution and the precipitant to obtain a two-dimensional flaky rare earth oxide.

[0031] Furthermore, the heat preservation reaction has a reaction temperature of 0 to 90° C. When the reaction temperature is 0 to 60° C., the thickness of the rare earth oxide flakes obtained is 30 to 100 nm, and when the reaction temperature is 60 to 90° C., the thickness of the rare earth oxide flakes obtained is 100 to 300 nm. By controlling the reaction temperature, the thickness of the rare earth oxide flakes can be adjusted.

[0032] Furthermore, after the reaction is completed, the pH value of the reaction solution is ≥8.

[0033] 2. The present invention discloses a nano-flaky rare earth oxide, which is prepared by the above method. The rare earth oxide is in the shape of a flake, and the thickness of the flake layer of the flake rare earth oxide is 30 to 300 nm.

[0034] The present invention will be further described below in conjunction with specific embodiments.

[0035] The structural morphology characterization process of the products prepared in the following embodiments and comparative examples is as follows: Sigma-500 scanning electron microscope (FESEM) is used for characterization. Before testing, the sample is placed at 60°C and dried for 1 hour before being used for test sample preparation. First, a conductive glue is pasted on the sample stage, a small amount of dry sample is taken on the conductive glue, and the excess sample outside the conductive glue is blown off with an ear bulb. Then, the sample stage is subjected to gold spraying treatment (30 to 90 seconds) on an ion sputtering coating instrument to increase the conductivity of the sample. After the gold plating is completed, a test voltage of 10kV is selected, and the sample stage is placed in the sample chamber for observation and imaging.

[0036] Example 1

[0037] Preparation of Nano-Flake Rare Earth Oxides:

[0038] (1) Prepare 100g / L lanthanum chloride solution. Prepare NH3 and CO3 2- The molar ratio is 1:2.3 and the concentration is 2 mol / L of carbonized ammonia aqueous solution.

[0039] (2) At 70°C, with water as the base liquid, the lanthanum chloride solution and the precipitant are simultaneously added dropwise to the base liquid for reaction, and the relative dropping rates of the lanthanum chloride solution and the precipitant solution are controlled to be 1:1.6, so that the molar ratio of lanthanum chloride to ammonium bicarbonate in the mixed precipitant solution is 1:3.2 during the dropping process. After the dropping is completed, the reaction is continued at 70°C for 0.5h.

[0040] (3) The reaction solution is filtered and the solid is washed with water to obtain a filter cake and a filtrate. The filter cake is dried to obtain a precursor. The precursor is calcined at 800°C for 2 hours to obtain nano-sheet lanthanum oxide. The SEM image of the nano-sheet lanthanum oxide is shown in Figure 2 The obtained nano-flaky lanthanum oxide has a sheet thickness of 130 to 190 nm.

[0041] Example 2

[0042] Preparation of Nano-Flake Rare Earth Oxides:

[0043] (1) Prepare 50g / L cerium chloride solution. Prepare NH3 and CO3 2- A carbonized ammonia aqueous solution with a molar ratio of 1:2.5 and a concentration of 1.8 mol / L.

[0044] (2) At 60° C., the cerium chloride solution and the mixed precipitant are simultaneously added dropwise to the base solution for reaction, and the relative dropping speed of the cerium chloride solution and the precipitant solution is controlled to be 1:1.8, so that the molar ratio of cerium chloride to ammonium bicarbonate in the mixed precipitant solution is 1:3.2 during the dropping process. After the dropping is completed, the reaction is continued at 60° C. for 0.5 h.

[0045] (3) The obtained reaction liquid is filtered and washed with water, and the filter cake is dried to obtain a precursor. The precursor is calcined at 800° C. for 2 h to obtain nano-sheet cerium oxide. The sheet thickness is 120 to 180 nm.

[0046] Example 3

[0047] The only difference from Example 1 is that the excess carbonized ammonia solution contains NH3 and CO3 2- The molar ratio is 1:2.5. The thickness of the obtained nano-flaky lanthanum oxide is 110-160 nm.

[0048] Example 4

[0049] The only difference from Example 1 is that the reaction temperature is 50° C. The thickness of the obtained nano-flaky lanthanum oxide is 65 to 90 nm.

[0050] Example 5

[0051] The only difference from Example 1 is that the molar ratio of lanthanum chloride to ammonium bicarbonate during the simultaneous dropwise addition of lanthanum chloride and the mixed precipitant solution is 1:2.5. The thickness of the obtained nano-flaky lanthanum oxide sheet is 157-200 nm.

[0052] Comparative Example 1

[0053] The difference from Example 1 is that the dropping method is that lanthanum chloride is added dropwise to the mixed precipitant solution, and the morphology of the obtained lanthanum oxide is a long strip aggregate. Figure 3 .

[0054] Comparative Example 2

[0055] The difference from Example 1 is that the NH3:CO3 2- The molar ratio is 1:1, and the morphology of the obtained lanthanum oxide is irregular block aggregates with poor dispersion. Figure 4 .

[0056] Comparative Example 3

[0057] The difference from Example 1 is that the relative dripping rate ratio of the rare earth solution and the precipitant is 1:3, and the morphology of the obtained oxide is micron-sized flake aggregates. Figure 5 .

[0058] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing nano-flaky rare earth oxides, characterized in that: The rare earth solution and an excess of carbonized ammonia water precipitant are simultaneously added dropwise to the bottom liquid for heat preservation reaction. After the reaction is completed, the precursor is calcined to obtain nano-sheet rare earth oxides.

2. The preparation method according to claim 1, characterized in that: The mass volume concentration of the rare earth solution is 10 to 320 g / L; 2- The molar concentration of the carbonized ammonia water precipitant is 1.5-2.3 mol / L.

3. The preparation method according to claim 1 or 2, characterized in that: NH3:CO3 in the carbonized ammonia precipitant 2- The molar ratio is 1:1.5~3.

5.

4. The preparation method according to claim 1, characterized in that: The RE of the rare earth solution and the carbonized ammonia precipitant solution 3+ :CO3 2- The molar ratio is 1:2.0~3.

5.

5. The preparation method according to claim 1, characterized in that: The relative dripping rate ratio of the rare earth solution and the carbonized ammonia water precipitant is 1:1.5-2.

0.

6. The preparation method according to claim 1, characterized in that: The rare earth solution is one or more of rare earth nitrate, rare earth chloride, rare earth sulfate and rare earth acetate.

7. The preparation method according to claim 1, characterized in that: The temperature of the heat preservation reaction is 0-90° C., the time is 0.5-1 h, and the calcination temperature is 700-900° C., the time is 1-4 h.

8. The preparation method according to claim 7, characterized in that: When the reaction temperature is 0-60°C, the thickness of the prepared rare earth oxide sheet is 30-100nm; when the reaction temperature is 60-90°C, the thickness of the prepared rare earth oxide sheet is 100-300nm.

9. The preparation method according to claim 1, characterized in that: After the reaction is completed, the pH value of the reaction solution is ≥8.

10. A nano-flaky rare earth oxide prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The thickness of the flaky rare earth oxide is 30-300 nm.