Method for preparing high-purity manganese carbonate

Through the reaction of sulfite with manganese sulfate solution and multi-step treatment, the problem of removing calcium and magnesium impurities in manganese sulfate was successfully solved, and high-purity manganese carbonate was prepared, which achieved high purity and low-cost production, avoiding environmental pollution and waste treatment. question.

CN118908280AActive Publication Date: 2024-11-08XIANGTAN UNIV +1

Patent Information

Application Number
CN202410944240.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-19
Filing Date
2024-07-15
Publication Date
2024-11-08
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove calcium and magnesium impurities in manganese sulfate solution, resulting in high calcium and magnesium content when preparing high-purity manganese carbonate, which cannot meet the high-purity standards. Common methods have problems such as difficulty in precipitation, strong corrosiveness, and pollution of the environment.

Method used

Precipitate with sulfite and industrial grade manganese sulfate solution. Through multiple steps, the treatment includes precipitation, filtration, rinsing, vacuum drying and acid dissolution. Manganese sulfite reacts with carbonate to prepare high-purity manganese carbonate to ensure calcium and magnesium impurities. Low content.

Benefits of technology

The preparation of high-purity manganese carbonate is achieved, with extremely low calcium and magnesium impurities, simple process and low cost, and no difficulty in dealing with waste generation, meeting the production requirements of high efficiency, low cost and green environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908280A_ABST
    Figure CN118908280A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing high-purity manganese carbonate, which comprises the following steps of: performing precipitation reaction on an industrial grade manganese sulfate solution and a solution containing sulfite ions by utilizing the property that the selectivity of sulfite to manganese is stronger than that of carbonate to calcium ions, so as to obtain manganese sulfite with extremely low calcium impurities, and then adding acid to dissolve the manganese sulfite, so as to obtain a solution containing manganese ions; and adding the carbonate ion-containing solution into the manganese ion-containing solution for precipitation reaction to obtain the high-purity manganese carbonate. The high-purity manganese carbonate prepared by the invention is simple in preparation process, low in production cost, green and environment-friendly, and the prepared high-purity manganese carbonate is low in impurity content of calcium and magnesium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-purity manganese-based material manufacturing, and in particular relates to a method for preparing high-purity manganese carbonate. Background Art

[0002] The application of manganese carbonate in the electronics, ceramics, chemical and pharmaceutical industries has attracted wide attention. High-purity manganese carbonate is an important material for the preparation of soft ferrites and lithium-ion power batteries, and its requirements on the impurity content of the raw materials are relatively strict. In the conventional preparation industry, high-purity manganese carbonate is mainly produced by the reaction of manganese sulfate solution and carbonate, but the manganese content of the sample is low, and the calcium and magnesium impurities are high, which is difficult to purify deeply.

[0003] At present, there are three main methods for purifying calcium ions and magnesium ions: variable temperature crystallization, chemical precipitation, and solvent extraction. The variable temperature crystallization of manganese sulfate solution is simple and easy to operate, but it is difficult to avoid the formation of mixed crystals of MnSO4, MgSO4, and CaSO4. Chemical precipitation is of great significance in the purification process of manganese salt solution. At present, the precipitation methods used in the preparation of high-purity manganese carbonate include fluoride precipitation, phosphate precipitation, and carbonate precipitation. In the chemical precipitation method, although fluoride ions can mask a small amount of calcium, the fluoride precipitation method cannot avoid the disadvantages of difficult precipitation, strong corrosiveness, and environmental pollution; while the loss of manganese is large when phosphate is used as a precipitant to remove calcium and manganese, and phosphogypsum is a hazardous waste, which is difficult to handle later and has great harm to the environment; carbonate has better selectivity for manganese than magnesium, but poorer selectivity for calcium. At the same time, the precipitation process is difficult to avoid the co-precipitation of calcium, magnesium, and manganese, so that the calcium and magnesium content in the prepared manganese carbonate still does not meet the standard requirements of high-purity manganese carbonate. Solvent extraction can be used to selectively separate manganese from other metals, avoiding the above-mentioned disadvantages of chemical precipitation, but the cost of reagents may limit its application to the removal of calcium and magnesium ions in manganese-containing solutions.

[0004] In recent years, with the rapid development of new energy, especially power batteries, the demand for high-quality manganese source manganese carbonate has increased dramatically. Therefore, a high-efficiency, low-cost method for preparing high-purity manganese carbonate suitable for large-scale production is urgently needed. Summary of the invention

[0005] In order to overcome the problems in the prior art, the present invention provides a method for preparing high-purity manganese carbonate. The method has a simple preparation process, low reagent cost, no difficult-to-treat waste generation, and the prepared high-purity manganese carbonate has low impurity content of calcium and magnesium.

[0006] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0007] The present invention provides a method for preparing high-purity manganese carbonate, comprising the following steps:

[0008] S1, subjecting an industrial-grade manganese sulfate solution to a precipitation reaction with a solution containing sulfite ions to obtain a slurry A;

[0009] S2, filtering the slurry A obtained in step S1 to obtain a filter residue;

[0010] S3, rinsing, filtering and vacuum drying the filter residue obtained in step S2 to obtain solid A;

[0011] S4, dissolving the solid A obtained in step S3 with acid to obtain a manganese ion-containing solution;

[0012] S5, subjecting the manganese ion-containing solution obtained in step S4 to a precipitation reaction with the carbonate ion-containing solution to obtain slurry B;

[0013] S6. The slurry B obtained in step S5 is filtered, rinsed, and then vacuum dried to obtain high-purity manganese carbonate.

[0014] The applicant has found that, relative to carbonate, sulfite is more selective to manganese than calcium and magnesium ions, and thus can be better used for the removal of calcium and magnesium in the process of manganese sulfate solution precipitation and removal of calcium and magnesium. The solubility product (Ksp) of manganese sulfite is small and the manganese content in manganese sulfate solution is high, so sulfite will first precipitate with manganese ions. In the present invention, sulfite is first reacted with industrial-grade manganese sulfate solution, and the slurry is filtered to obtain a filter residue, and the filter residue is rinsed to wash away the sulfate remaining in the filter residue, and vacuum drying (to prevent the sample from being oxidized) after filter pressing can obtain solid A, i.e., manganese sulfite solid, and then manganese sulfite is dissolved by acid to obtain a manganese ion solution, and after reacting with carbonate, high-purity manganese carbonate can be obtained.

[0015] As an optional embodiment, in the preparation method provided by the present invention, in step S1, the concentration of manganese ions in the industrial-grade manganese sulfate solution is 18 to 75 g / L, the pH value is 2 to 8, and the amount of the solution containing sulfite ions is 0.8 to 1.5 times the amount used for complete precipitation of the industrial-grade manganese sulfate solution.

[0016] In the present invention, the pH of the industrial-grade manganese sulfate solution is adjusted to 2-8. If the pH is too high, manganese ions will be oxidized, and if the pH is too low, there will be excessive loss of sulfite.

[0017] As an optional embodiment, in the preparation method provided by the present invention, in step S1, the calcium ion concentration in the industrial-grade manganese sulfate solution is 0.09-0.39 g / L, and the magnesium ion concentration is 0.12-0.52 g / L.

[0018] As an optional embodiment, in the preparation method provided by the present invention, the solution containing sulfite ions is selected from one or more of ammonium sulfite, ammonium bisulfite, sodium sulfite, and sodium bisulfite solutions, and the sulfite concentration in the solution is 10 to 400 g / L.

[0019] As an optional embodiment, in the preparation method provided by the present invention, the process of the precipitation reaction in step S1 is to add a solution containing sulfite ions to a manganese sulfate solution, control the feeding rate of the sulfite solution to be 2 to 10 ml / min, the stirring rate to be 200 to 400 r / min, the stirring time to be 1 to 6 h, and the reaction temperature to be 10 to 60 ° C.

[0020] In the present invention, the addition rate of the sulfite solution is controlled to be 2-10 ml / min, which can ensure the sufficiency of the reaction. The faster the addition rate, the faster the precipitation will be formed, and a large amount of calcium and magnesium impurities will be wrapped, affecting the purity of the product. The reaction temperature is set to 10-60°C, which is conducive to the reaction. Too low a temperature will cause the high-concentration manganese sulfate solution to crystallize and precipitate, resulting in an incomplete reaction. Too high a temperature will affect the product yield.

[0021] As an optional embodiment, in the preparation method provided by the present invention, a filtrate is obtained after filtration in step S2, and the filtrate is used to produce an ammonium sulfate product.

[0022] The filtrate in the present invention is an ammonium sulfate solution containing calcium and magnesium. Since the calcium and magnesium contents in industrial-grade manganese sulfate are relatively low, the ammonium sulfate filtrate can be used to produce ammonium sulfate products, such as fertilizers.

[0023] As an optional embodiment, in the preparation method provided by the present invention, in step S4, the acid is sulfuric acid with a concentration of 0.1 to 4 mol / L.

[0024] As an optional embodiment, in the preparation method provided by the present invention, in step S4, the sulfur dioxide gas generated during the acid dissolution process is collected to prepare a sulfite solution, and the obtained sulfite solution is reused in step S1 as a reaction raw material.

[0025] As an optional embodiment, in the preparation method provided by the present invention, in step S4, the concentration of manganese ions in the manganese ion-containing solution is 18-70 g / L.

[0026] In the present invention, the concentration of manganese ions in the manganese ion-containing solution is 18-70 g / L. If the concentration is lower than this, the impurity removal effect cannot be achieved and the calcium and magnesium impurity contents of the product are too high.

[0027] As an optional embodiment, in the preparation method provided by the present invention, in step S5, the carbonate ion-containing solution is selected from one or more of ammonium bicarbonate, ammonium carbonate, sodium carbonate, and sodium bicarbonate.

[0028] As an optional embodiment, in the preparation method provided by the present invention, in step S5, the amount of the carbonate ion-containing solution used is 0.8 to 1.2 times the theoretical amount of the manganese ion-containing solution used for complete precipitation.

[0029] In the present invention, the amount of carbonate ion used is lower than the theoretical value, which is beneficial for calcium and magnesium to remain in the solution, reducing the calcium and magnesium impurity content in manganese sulfite, and the purity of manganese sulfite is higher; higher than the theoretical value is beneficial to ensure the precipitation rate of manganese; and qualified products can be prepared between 0.8 and 1.2.

[0030] As an optional embodiment, in the preparation method provided by the present invention, the process of the precipitation reaction in step S5 is to control the initial pH value of the reaction of the manganese ion solution and the carbonate ion solution to be 4-8, and the carbonate ion solution is added to the manganese ion solution. The feeding rate of the carbonate solution is 2-10 ml / min, the stirring rate is 200-400 r / min, the stirring time is 1-6 h, and the reaction temperature is set to 10-60 ° C.

[0031] As an optional embodiment, in the preparation method provided by the present invention, in step S3, the vacuum drying temperature is 60 to 120° C., and the drying time is 4 to 24 hours.

[0032] As an optional embodiment, in the preparation method provided by the present invention, in step S6, the vacuum drying temperature is 60 to 120° C., and the drying time is 4 to 24 hours.

[0033] As an optional embodiment, in the preparation method provided by the present invention, the manganese content in the high-purity manganese carbonate is higher than 45%, the calcium content is less than 100 ppm, and the magnesium content is less than 30 ppm.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] In the present invention, manganese sulfite is used as an intermediate product, and high-purity manganese sulfate is obtained after acid dissolution, and then combined with a carbonate solution for precipitation reaction to obtain a high-purity manganese carbonate product with extremely low calcium and magnesium impurity content. The process of the present invention is simple, and the purity of the obtained manganese carbonate is extremely high. The production process is green and environmentally friendly, and no difficult-to-treat waste is generated. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0038] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0039] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0040] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0041] Example 1

[0042] A method for preparing high-purity manganese carbonate based on manganese sulfite, the process flow chart is as follows Figure 1 As shown, the following steps are included:

[0043] (1) Weigh an industrial-grade manganese sulfate sample, dissolve it in water, and prepare 100 ml of a manganese sulfate solution having a manganese ion concentration of 36 g / L, a calcium ion concentration of 0.19 g / L, and a magnesium ion concentration of 0.25 g / L, and adjust the pH to 2; weigh 11.5 g of ammonium sulfite, dissolve it in water, and prepare 100 ml of an ammonium sulfite solution.

[0044] (2) Under the conditions of a temperature of 10° C. and a stirring rate of 300 r / min, the ammonium sulfite solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 3 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 1.5 h to obtain slurry A.

[0045] (3) Slurry A is filtered by a vacuum circulation pump to separate solid from liquid. The solid residue is rinsed with pure water and filtered three times to obtain manganese sulfite. The obtained manganese sulfite is dried in a vacuum drying oven at 60° C. for 10 h. The filtrate is recovered and used to produce ammonium sulfate products.

[0046] (4) 5 g of vacuum-dried manganese sulfite solid was taken, 1 mol / L dilute sulfuric acid was added to dissolve it to obtain a manganese sulfate solution, and the obtained manganese sulfate solution was diluted to 100 ml with water, and the pH was adjusted to 4; 4.13 g of ammonium bicarbonate was weighed, and water was added to dissolve it to prepare 100 ml of ammonium bicarbonate solution.

[0047] (5) Under the conditions of a temperature of 10° C. and a stirring rate of 300 r / min, the ammonium bicarbonate solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 3 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 1.5 h to obtain slurry B.

[0048] (6) The slurry B was filtered by a vacuum circulation pump to separate the solid and liquid. The filter residue was rinsed with pure water and filtered three times, and dried in a vacuum drying oven at 60° C. for 10 h to obtain high-purity manganese carbonate.

[0049] Example 2

[0050] A method for preparing high-purity manganese carbonate based on manganese sulfite comprises the following steps:

[0051] (1) Weigh an industrial-grade manganese sulfate sample, dissolve it in water, and prepare 100 ml of a manganese sulfate solution having a manganese ion concentration of 36 g / L, a calcium ion concentration of 0.19 g / L, and a magnesium ion concentration of 0.25 g / L, and adjust the pH to 4.5; weigh 7.7 g of ammonium sulfite, dissolve it in water, and prepare 200 ml of an ammonium sulfite solution.

[0052] (2) Under the conditions of a temperature of 25° C. and a stirring rate of 300 r / min, the ammonium sulfite solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 3 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 1.5 h to obtain slurry A.

[0053] (3) Slurry A is filtered by a vacuum circulation pump to separate solid from liquid, and the solid residue is rinsed with pure water and filtered three times to obtain manganese sulfite, which is then dried in a vacuum drying oven at 80° C. for 10 h. The filtrate is recovered and used to produce ammonium sulfate products.

[0054] (4) 5 g of vacuum-dried manganese sulfite solid was taken, 1 mol / L dilute sulfuric acid was added to dissolve it to obtain a manganese sulfate solution, and the obtained manganese sulfate solution was diluted to 100 ml with water, and the pH was adjusted to 7; 5.16 g of ammonium bicarbonate was weighed, and water was added to dissolve it to prepare 100 ml of ammonium bicarbonate solution.

[0055] (5) At a temperature of 25° C. and a stirring rate of 300 r / min, the ammonium bicarbonate solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 3 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 1.5 h to obtain slurry B.

[0056] (6) The slurry B was filtered by a vacuum circulation pump to separate the solid and liquid. The filter residue was rinsed with pure water and filtered three times, and dried in a vacuum drying oven at 80° C. for 10 h to obtain high-purity manganese carbonate.

[0057] Example 3

[0058] A method for preparing high-purity manganese carbonate based on manganese sulfite comprises the following steps:

[0059] (1) Weigh an industrial-grade manganese sulfate sample, dissolve it in water, and prepare 100 ml of a manganese sulfate solution having a manganese ion concentration of 75 g / L, a calcium ion concentration of 0.39 g / L, and a magnesium ion concentration of 0.52 g / L, and adjust the pH to 6; weigh 13.8 g of sodium sulfite, dissolve it in water, and prepare 100 ml of a sodium sulfite solution.

[0060] (2) Under the conditions of a temperature of 25° C. and a stirring rate of 400 r / min, the sodium sulfite solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 2 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 3 h, thereby obtaining slurry A.

[0061] (3) Slurry A is filtered by a vacuum circulation pump to separate solid from liquid. The solid residue is rinsed with pure water and filtered three times to obtain manganese sulfite. The obtained manganese sulfite is dried in a vacuum drying oven at 80° C. for 16 h. The filtrate is recovered and used to produce ammonium sulfate products.

[0062] (4) 10 g of vacuum-dried manganese sulfite solid was taken, 1 mol / L dilute sulfuric acid was added to dissolve it to obtain a manganese sulfate solution, and the obtained manganese sulfate solution was diluted to 100 ml with water, and the pH was adjusted to 4; 14.0 g of ammonium bicarbonate was weighed, and water was added to dissolve it to prepare 100 ml of ammonium bicarbonate solution.

[0063] (5) At a temperature of 25° C. and a stirring rate of 300 r / min, the ammonium bicarbonate solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 2 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 3 h, thereby obtaining slurry B.

[0064] (6) The slurry B was filtered by a vacuum circulation pump to separate the solid and liquid. The filter residue was rinsed with pure water and filtered three times, and dried in a vacuum drying oven at 60° C. for 16 h to obtain high-purity manganese carbonate.

[0065] Example 4

[0066] A method for preparing high-purity manganese carbonate based on manganese sulfite comprises the following steps:

[0067] (1) Weigh an industrial-grade manganese sulfate sample, dissolve it in water, and prepare 200 ml of a manganese sulfate solution having a manganese ion concentration of 27 g / L, a calcium ion concentration of 0.14 g / L, and a magnesium ion concentration of 0.19 g / L, and adjust the pH to 8; weigh 23.1 g of ammonium sulfite, dissolve it in water, and prepare 200 ml of an ammonium sulfite solution.

[0068] (2) Under the conditions of a temperature of 60° C. and a stirring rate of 300 r / min, the ammonium sulfite solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 10 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 1.5 h to obtain slurry A.

[0069] (3) Slurry A is filtered by a vacuum circulation pump to separate solid from liquid. The solid residue is rinsed with pure water and filtered three times to obtain manganese sulfite. The obtained manganese sulfite is dried in a vacuum drying oven at 60° C. for 24 hours. The filtrate is recovered and used to produce ammonium sulfate products.

[0070] (4) 10 g of vacuum-dried manganese sulfite solid was taken, 1 mol / L dilute sulfuric acid was added to dissolve it to obtain a manganese sulfate solution, and the obtained manganese sulfate solution was diluted to 100 ml with water, and the pH was adjusted to 8; 11.7 g of ammonium bicarbonate was weighed, and water was added to dissolve it to prepare 100 ml of ammonium bicarbonate solution.

[0071] (5) At a temperature of 60° C. and a stirring rate of 300 r / min, the ammonium bicarbonate solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 10 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 1.5 h to obtain slurry B.

[0072] (6) The slurry B was filtered by a vacuum circulation pump to separate the solid and liquid. The filter residue was rinsed with pure water and filtered three times, and dried in a vacuum drying oven at 60° C. for 24 h to obtain high-purity manganese carbonate.

[0073] Comparative Example 1

[0074] (1) Weigh an industrial-grade manganese sulfate sample, dissolve it in water, and prepare 100 ml of a manganese sulfate solution having a manganese ion concentration of 36 g / L, a calcium ion concentration of 0.19 g / L, and a magnesium ion concentration of 0.25 g / L, and adjust the pH to 4.5; weigh 10.4 g of ammonium bicarbonate, dissolve it in water, and prepare 200 ml of an ammonium bicarbonate solution.

[0075] (2) Under the conditions of a temperature of 25° C. and a stirring rate of 300 r / min, the ammonium bicarbonate solution was delivered to the manganese sulfate solution through a delivery pump at a rate of 3 ml / min. After the delivery was completed, stirring was continued and the total reaction time was controlled to be 1.5 h to obtain slurry A.

[0076] (3) Slurry A was filtered by a vacuum circulation pump to separate solid from liquid. The solid residue was rinsed with pure water and filtered for three times to obtain manganese carbonate. The obtained manganese carbonate was dried in a vacuum drying oven at 80° C. for 10 h.

[0077] The manganese sulfite prepared in the example and the manganese carbonate prepared in the example and the comparative example were tested for the contents of manganese, calcium and magnesium. The ICP test results of the specific contents are shown in Table 1:

[0078] Table 1: Content test results

[0079]

[0080] In the industrial-grade manganese sulfate solid used in the experiment, the calcium content is 1920ug / g, and the magnesium content is 2500ug / g. As can be seen from Table 1, the calcium content in the intermediate product manganese sulfite has been reduced to below 100ug / g, and the removal rate can reach 98%, and the magnesium content is reduced to below 350ug / g, and the removal rate can reach 86%, indicating that the calcium and magnesium contents in the precipitated solid can be significantly reduced by using sulfite as a precipitant to precipitate manganese. The high-purity manganese carbonate prepared with manganese sulfite as the intermediate product has a manganese content higher than the enterprise standard, and the calcium and magnesium contents are far lower than the enterprise standard, indicating that the method has produced a high-purity manganese carbonate product with low calcium and magnesium. In summary, the high-purity manganese carbonate prepared according to the method of the present invention has a manganese content that meets the standard requirements of high-purity manganese carbonate, and the calcium and magnesium impurity contents are far lower than the standard requirements.

[0081] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A method for preparing high-purity manganese carbonate, characterized in that: The following steps are involved: S1, subjecting an industrial-grade manganese sulfate solution to a precipitation reaction with a solution containing sulfite ions to obtain a slurry A; S2, filtering the slurry A obtained in step S1 to obtain a filter residue; S3, rinsing, filtering and vacuum drying the filter residue obtained in step S2 to obtain solid A; S4, dissolving the solid A obtained in step S3 with acid to obtain a manganese ion-containing solution; S5, subjecting the manganese ion-containing solution obtained in step S4 to a precipitation reaction with the carbonate ion-containing solution to obtain slurry B; S6. The slurry B obtained in step S5 is filtered, rinsed, and then vacuum dried to obtain high-purity manganese carbonate.

2. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: In step S1, the concentration of manganese ions in the industrial-grade manganese sulfate solution is 18-75 g / L, the pH value is 2-8, and the amount of the solution containing sulfite ions is 0.8-1.5 times the amount of the industrial-grade manganese sulfate solution used for complete precipitation.

3. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: In step S1, the calcium ion concentration in the industrial-grade manganese sulfate solution is 0.09-0.39 g / L, and the magnesium ion concentration is 0.12-0.52 g / L.

4. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: The solution containing sulfite ions is selected from one or more of ammonium sulfite, ammonium bisulfite, sodium sulfite and sodium bisulfite solutions, and the concentration of sulfite in the solution is 10-400 g / L.

5. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: The process of the precipitation reaction in step S1 is to add the solution containing sulfite ions into the manganese sulfate solution, control the feeding rate of the sulfite solution to be 2-10 ml / min, the stirring rate to be 200-400 r / min, the stirring time to be 1-6 h, and the reaction temperature to be 10-60° C.

6. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: After filtering in step S2, a filtrate is obtained, which is used to produce an ammonium sulfate product.

7. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: In step S4, the acid is sulfuric acid with a concentration of 0.1-4 mol / L; the sulfur dioxide gas generated during the acid dissolution process is collected to prepare a sulfite solution, and the obtained sulfite solution is reused in step S1 as a reaction raw material.

8. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: The precipitation reaction process in step S5 is to control the initial pH value of the manganese ion solution to be 4-8, add the carbonate ion solution to the manganese ion solution, add the carbonate solution at a rate of 2-10 ml / min, stir at a rate of 200-400 r / min, stir for 1-6 h, and set the reaction temperature to 10-60° C.; The amount of the carbonate ion solution is 0.8 to 1.2 times the theoretical amount of the manganese ion solution for complete precipitation; the carbonate ion solution is selected from one or more of ammonium bicarbonate, ammonium carbonate, sodium carbonate, and sodium bicarbonate; In step S6, the vacuum drying temperature is 60 to 120° C., and the drying time is 4 to 24 hours.

9. The method for preparing high-purity manganese carbonate according to claim 1, characterized in that: The manganese content in high-purity manganese carbonate is higher than 45%, the calcium content is less than 100ppm, and the magnesium content is less than 30ppm.

Citation Information

Patent Citations

  • Method for preparing high purity manganese carbonate

    CN105036197A

  • Method for simultaneously preparing manganese sulfide and battery grade manganese sulfate

    CN116534900A

Cited By

  • Method for oxidizing and separating manganese and magnesium and preparing basic magnesium carbonate by using manganese dioxide as catalyst

    CN119797434A