Method for preparing battery-grade high-purity high-tap-density manganous-manganic oxide from manganese sulfate solution and application of battery-grade high-purity high-tap-density manganous-manganic oxide

By adding surfactant and ammonia precipitation to manganese sulfate solution, and using compaction molding and oxidation and roasting processes, the problems of low conversion rate and unstable quality in the manganese sulfate solution method were solved, and high-purity and high-tap density were successfully prepared. Trimanganese tetraoxide meets the needs of battery-grade products.

CN118908281AInactive Publication Date: 2024-11-08CENT SOUTH UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410948765.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing manganese sulfate solution method has low conversion rate, low product tap density and unstable quality, making it difficult to meet the market's demand for high-purity trimanganese tetraoxide products.

Method used

After the precipitation reaction is carried out by adding surfactant and ammonia water to manganese sulfate solution, it is washed, dried, added binder and applied pressure to compact and molded, followed by oxidation and roasting to obtain high-purity, high-tap density tetraoxide Trimanganese.

Benefits of technology

The tap density and purity of trimanium tetraoxide are improved, the problems of low conversion rate and unstable quality are solved, and high-quality battery-grade trimanium tetraoxide products are obtained, which are easy to operate and efficient in process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908281A_ABST
    Figure CN118908281A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing battery-grade high-purity and high-tap-density manganous-manganic oxide from a manganese sulfate solution and application of the manganous-manganic oxide, and the method comprises the following steps: adding a surfactant into the manganese sulfate solution, heating, continuously stirring, slowly adding ammonia water to carry out precipitation reaction, cooling to room temperature after the reaction is finished, and carrying out solid-liquid separation to obtain a precipitate; washing the precipitate with deionized water, and drying; adding a certain amount of binder into the dried precipitate, and applying pressure for compaction molding to obtain a molded material; and roasting the formed material, cooling, crushing and screening to obtain a manganous-manganic oxide product. The method solves the problems of low conversion efficiency, low product tap density, unstable quality and the like in the traditional manganese sulfate solution method, and has the advantages of simplicity and convenience in operation and high process efficiency, and the tap density of the prepared high-quality battery-grade manganous-manganic oxide is up to 2.88 g / cm < 3 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium manganate positive electrode materials, and in particular to a method for preparing battery-grade high-purity and high-tap density manganese tetraoxide from a manganese sulfate solution and application thereof. Background Art

[0002] Among lithium-ion power batteries, lithium manganese oxide batteries with lithium manganese oxide as the positive electrode material are widely used because of their advantages such as low production cost, good low temperature performance and high safety performance. The production of lithium manganese oxide mainly uses electrolytic manganese dioxide as the manganese source, which has disadvantages such as high cost, high impurity content and poor cycle performance. Compared with manganese dioxide and other manganese sources, the impurity ion content in manganese tetraoxide, especially the impurity sulfur content, is lower, and manganese tetraoxide has the same spinel structure as lithium manganese oxide, and the structural stability of the phase change process is better. The synthesis of lithium manganese oxide using manganese tetraoxide as the manganese source has been significantly improved in terms of high temperature cycle performance and production cost. Therefore, manganese tetraoxide stands out in the field of preparing lithium-ion battery materials and is a high-quality raw material for synthesizing positive electrode material lithium manganese oxide.

[0003] At present, the preparation of battery-grade manganese tetraoxide in the industry can be roughly divided into two directions: low-valent manganese oxidation and high-valent manganese reduction, mainly including metallic manganese suspension oxidation method and manganese sulfate solution method.

[0004] The metal manganese suspension oxidation method refers to the use of electrolytic metal manganese flakes as raw materials, crushing them into a suspension, using ammonium salt as a catalyst, and then introducing oxygen or air under certain temperature conditions for oxidation, thereby preparing manganese tetraoxide. This method is simple in process and has a high yield. Most battery-grade manganese tetraoxide produced by domestic manufacturers is prepared by the metal manganese method, but this method is limited by raw materials, the price of electrolytic metal manganese flakes is expensive, and the prepared manganese tetraoxide product has a high content of iron and sulfur impurities, which will affect the performance of lithium manganate products.

[0005] The manganese sulfate solution method refers to the process of using manganese sulfate solution as raw material, adding ammonia water or other alkaline solution to a certain concentration of manganese sulfate solution to generate manganese hydroxide precipitate, and then oxidizing the precipitate to manganese tetraoxide using air. This method can effectively reduce the cost of raw materials, but due to the long reaction time, low conversion rate of manganese tetraoxide, low product tap density, and unstable quality, it is difficult to meet the market demand for battery-grade high-purity manganese tetraoxide products.

[0006] The alkalization precipitation-roasting process can improve some of the shortcomings of the manganese sulfate solution method. The manganese sulfate solution is precipitated with alkali solution, and then precipitated by oxidation roasting to obtain manganese tetraoxide, which can effectively improve the oxidation efficiency. However, this process still has problems such as low process conversion rate, low tap density of the prepared manganese tetraoxide, irregular particle morphology, and poor uniformity of particle size. Therefore, a more effective method is needed to solve the shortcomings of the above process. Summary of the invention

[0007] The present invention provides a method for preparing battery-grade high-purity and high-tap density manganese tetraoxide from a manganese sulfate solution and its application, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0008] In order to achieve the above object, an embodiment of the present invention provides a method for preparing battery-grade high-purity, high-tap density manganese tetraoxide from a manganese sulfate solution, comprising the following steps:

[0009] S1: adding a surfactant to the manganese sulfate solution, heating, continuously stirring and slowly adding ammonia water to perform a precipitation reaction, and after the reaction is completed and cooled to room temperature, performing solid-liquid separation to obtain a precipitate;

[0010] S2: washing the precipitate with deionized water and drying;

[0011] S3: adding a certain amount of binder to the dried precipitate, and applying pressure to compact and shape it to obtain a molding material;

[0012] S4: calcining the molding material, cooling, crushing and screening to obtain the trimanganese tetraoxide product.

[0013] According to one aspect of the embodiments of the present invention, in step S1, the concentration of the sulfuric acid solution is 0.2-1.5 mol / L; the concentration of the ammonia water is 10%-15%; and the surfactant is cetyltrimethylammonium bromide (CTAB) with a concentration of 0.5-5.0 g / L.

[0014] According to one aspect of the embodiments of the present invention, in step S1, the heating temperature is 50-80°C; the stirring rate is 300-500 r / min; the ammonia addition time is 6-10 hours; and after the ammonia is completely added, the reaction is continued for 4-12 hours.

[0015] According to one aspect of the embodiments of the present invention, in step S2, the drying temperature is 40-80° C., and the drying time is 8-15 hours.

[0016] According to one aspect of the embodiments of the present invention, in step S3, the binder is carboxymethyl cellulose (CMC), polyacrylamide (PAM) or starch.

[0017] According to one aspect of the embodiment of the present invention, in step S3, the pressure is 5-100 MPa.

[0018] According to one aspect of the embodiments of the present invention, in step S3, the molding material is agglomerates or particles.

[0019] According to one aspect of the embodiment of the present invention, in step S4, the calcination temperature is 900-1150° C., and the calcination time is 1-4 hours.

[0020] According to one aspect of an embodiment of the present invention, in step S4, the tap density of trimanganese tetraoxide is as high as 2.88 g / cm 3 .

[0021] The embodiments of the present invention also provide the use of manganese tetraoxide prepared by the above method in a battery.

[0022] Mechanism description

[0023] The present invention uses compaction molding to process the dried precipitate, and by adding a binder, a molding material with a higher density is obtained, and the tap density of manganese tetraoxide is further increased by subsequent oxidation roasting. Through the molding process, the powder material is rearranged under the action of external force, the contact surface is increased, the interaction force between particles is enhanced, the porosity is reduced, the strength and density of the material are improved, and finally a molding agglomerate with strength and density is obtained. Compared with the powder material, the original density of the block material after molding is increased, the material is in a dense accumulation state, the contact area between particles is larger, the internal uniformity is better, the uniform distribution of the thermal field inside the material and between the material layers makes the block temperature distribution more uniform, the larger contact points between the particles promote better heat energy transfer through solid bridging, the heat transfer efficiency is increased, and the improvement of the permeability of the material layer and the heat transfer process is conducive to enhancing the gas-solid reaction kinetic conditions. In the subsequent oxidation roasting stage, the stable permeability of the material layer can effectively improve the oxygen kinetic transfer, the rapid mass transfer and heat transfer increase the thermal driving force, make the grain nucleation easier, promote the crystal transformation process, effectively improve the conversion efficiency of the precipitation, improve the microstructure of manganese tetraoxide, and obtain high tap density manganese tetraoxide with a stable lattice structure.

[0024] The above scheme of the present invention has the following beneficial effects:

[0025] (1) The present invention utilizes an alkali solution to precipitate a manganese sulfate solution, and compacts the dried precipitate into a shape, and obtains a battery-grade manganese tetraoxide with high purity and high tap density after calcination, thereby solving the problems of low conversion efficiency, low product tap density, and unstable quality existing in the traditional manganese sulfate solution method. The method is simple to operate, has an efficient process, and can obtain a high-quality battery-grade manganese tetraoxide product.

[0026] (2) The present invention uses a compaction and roasting process to compact the dried precipitate under the action of a binder, which can effectively improve oxygen kinetic transfer, increase the air permeability of the material layer of the formed agglomerate, and regulate the oxidation behavior of the precipitate, thereby achieving the effect of improving the process conversion rate and the tap density of manganese tetraoxide.

[0027] (3) After the molded agglomerates in the present invention are calcined at high temperature, sulfur is removed more thoroughly and the agglomerates are fully oxidized. Therefore, the obtained trimanganese tetraoxide has a lower sulfur content and a higher manganese content, and the product composition is high in purity and stable in quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 It is a schematic flow chart of a method for preparing battery-grade high-purity, high-tap-density trimanganese tetraoxide from a manganese sulfate solution according to one embodiment of the present invention;

[0030] Figure 2 It is a comparison chart of the X-ray diffraction analysis spectrum of trimanganese tetraoxide prepared in one embodiment of the present invention and the standard spectrum;

[0031] Figure 3 This is a microscopic morphology of manganese tetraoxide prepared in one embodiment of the present invention;

[0032] Figure 4 The invention discloses an embodiment of a method for preparing battery-grade high-purity, high-tap-density manganese tetraoxide from a manganese sulfate solution, and discloses an effect of molding pressure on the apparent density of a molded agglomerate;

[0033] Figure 5 It is a comparison chart of the tap density and manganese content of trimanganese tetraoxide prepared by Comparative Examples 1-4 and Examples 1-5 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0035] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0036] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0037] In view of the existing problems, the present invention provides a method for preparing battery-grade high-purity and high-tap density manganese tetraoxide from manganese sulfate solution. The schematic flow chart is as follows: Figure 1 As shown, the following steps are included:

[0038] S1: adding a surfactant to the manganese sulfate solution, heating, continuously stirring and slowly adding ammonia water to perform a precipitation reaction, and after the reaction is completed and cooled to room temperature, performing solid-liquid separation to obtain a precipitate;

[0039] S2: washing the precipitate with deionized water and drying;

[0040] S3: adding a certain amount of binder to the dried precipitate, and applying pressure to compact and shape it to obtain a molding material;

[0041] S4: calcining the molding material, cooling, crushing and screening to obtain the trimanganese tetraoxide product.

[0042] According to one aspect of the embodiments of the present invention, in step S1, the concentration of the sulfuric acid solution is 0.2-1.5 mol / L; the concentration of the ammonia water is 10%-15%; and the surfactant is cetyltrimethylammonium bromide (CTAB) with a concentration of 0.5-5.0 g / L.

[0043] According to one aspect of the embodiments of the present invention, in step S1, the heating temperature is 50-80°C; the stirring rate is 300-500 r / min; the ammonia addition time is 6-10 hours; and after the ammonia is completely added, the reaction is continued for 4-12 hours.

[0044] According to one aspect of the embodiments of the present invention, in step S2, the drying temperature is 40-80° C., and the drying time is 8-15 hours.

[0045] According to one aspect of the embodiments of the present invention, in step S3, the binder is carboxymethyl cellulose (CMC), polyacrylamide (PAM) or starch.

[0046] According to one aspect of the embodiment of the present invention, in step S3, the pressure is 5-100 MPa.

[0047] According to one aspect of the embodiments of the present invention, in step S3, the molding material is agglomerates or particles.

[0048] According to one aspect of the embodiment of the present invention, in step S4, the calcination temperature is 900-1150° C., and the calcination time is 1-4 hours.

[0049] According to one aspect of an embodiment of the present invention, in step S4, the tap density of trimanganese tetraoxide is as high as 2.88 g / cm 3 .

[0050] The following will describe the invention through specific embodiments.

[0051] Example 1

[0052] A method for preparing battery-grade high-purity, high-tap density manganese tetraoxide from a manganese sulfate solution comprises the following steps:

[0053] (1) Add 1 g / L of surfactant CTAB to a 0.5 mol / L high-purity manganese sulfate solution, heat to 65°C, control the stirring rate to 300 r / min, slowly drop ammonia water (mass fraction 15%) into the high-purity manganese sulfate solution at a dropping speed of 2.0 mL / min, and the pH value is 9.0-9.4. After the ammonia water is completely added, continue stirring for 6 h to ensure that the reaction is complete.

[0054] (2) After the solution system is stable, stop heating, cool the solution to room temperature, and filter to obtain a precipitate. Wash the precipitate with deionized water three times, and dry it in a vacuum drying oven at 80°C for 6 hours.

[0055] (3) A certain amount of carboxymethyl cellulose (CMC) is added to the dried precipitate and mixed evenly, and a pressure of 45 MPa is applied during the compaction molding process to prepare a molded mass.

[0056] (4) The agglomerate was calcined at 950°C for 2 hours, and then crushed after cooling to obtain high-purity manganese tetraoxide. The tap density of the manganese tetraoxide was 2.79 g / cm 3 , the manganese content is 70.51%.

[0057] Example 2

[0058] The method is the same as that in Example 1, except that a certain amount of polyacrylamide (PAM) is added to the dried precipitate, the pressure applied during the compaction molding process is 45 MPa, and other conditions remain unchanged. The tap density of the obtained manganese tetraoxide is 2.68 g / cm 3 , the manganese content is 70.48%.

[0059] Example 3

[0060] The method is the same as that in Example 1, except that a certain amount of starch is added to the dried precipitate and mixed evenly, and the pressure applied during the compaction molding process is 45 MPa, while other conditions remain unchanged. The tap density of the obtained manganese tetraoxide is 2.88 g / cm 3 , the manganese content is 70.98%.

[0061] Example 4

[0062] The method is the same as that in Example 3, except that the pressure applied during the compaction molding process is 15 MPa, and other conditions remain unchanged. The tap density of the obtained trimanganese tetraoxide is 2.55 g / cm 3 , the manganese content is 70.65%.

[0063] Example 5

[0064] The method is the same as that in Example 3, except that a certain amount of starch is added to the dried precipitate and mixed evenly, and the pressure applied during the compaction molding process is 60 MPa, while other conditions remain unchanged. The tap density of the obtained manganese tetraoxide is 2.61 g / cm 3 , the manganese content is 70.73%.

[0065] Comparative Example 1

[0066] (1) Add 1 g / L of surfactant CTAB to a 0.5 mol / L high-purity manganese sulfate solution, heat to 65°C, control the stirring rate to 300 r / min, slowly drop ammonia water (mass fraction 15%) into the high-purity manganese sulfate solution at a dropping speed of 2.0 mL / min, and the pH value is 9.0-9.4. After the ammonia water is completely added, continue stirring for 6 h to ensure that the reaction is complete.

[0067] (2) After the solution system is stable, stop heating, cool the solution to room temperature, and filter to obtain a precipitate. Wash the precipitate with deionized water three times, and dry it in a vacuum drying oven at 80°C for 6 hours.

[0068] (3) The dried precipitate was calcined at 950°C for 2 hours, and then crushed after cooling to obtain high-purity manganese tetraoxide. The tap density of the manganese tetraoxide is 2.22 g / cm 3 , the manganese content is 70.25%.

[0069] Comparative Example 2

[0070] The method is the same as that of Comparative Example 1, except that the dried precipitate is calcined by microwave calcination at 900°C, and other conditions remain unchanged. The tap density of the obtained manganese tetraoxide is 2.30 g / cm 3 , the manganese content is 70.12%.

[0071] Comparative Example 3

[0072] The method is the same as that of Example 3, except that the pressure applied during the compaction molding process is 110 MPa, and other conditions remain unchanged. The tap density of the obtained trimanganese tetraoxide is 2.16 g / cm 3 , the manganese content is 70.46%.

[0073] Comparative Example 4

[0074] The method is the same as that in Example 3, except that a certain amount of humic acid is added to the dried precipitate and mixed evenly. The tap density of the manganese tetraoxide is 2.34 g / cm 3 , the manganese content is 69.57%.

[0075] application

[0076] The manganese tetraoxide prepared in Example 3 is used as a manganese source to synthesize the positive electrode material. Its purity, impurity content and morphology have an important influence on the performance of the battery positive electrode material. In addition, the tap density of manganese tetraoxide directly affects the energy density, cycle stability and safety performance of the battery.

[0077] Table 1 Analysis of element contents in the manganese tetraoxide product prepared in Example 3

[0078]

[0079] Table 2 Physical properties of manganese tetraoxide products prepared in Example 3

[0080]

[0081] Table 1 is an analysis of the element content in the trimanganese tetroxide product prepared in Example 3. It can be seen from Table 1 that the trimanganese tetroxide prepared by the present invention has a high manganese content, and the content of impurity elements meets the industry standard, and is a high-purity trimanganese tetroxide product.

[0082] Table 2 shows the physical properties of the manganese tetraoxide product prepared in Example 3. It can be seen from Table 2 that the manganese tetraoxide prepared by the present invention has a uniform particle size distribution. 10 , D 50 and D 90 The relevant particle size indicators meet the industry standards, and the tap density is as high as 2.88g / cm 3 , the specific surface area also meets the standards.

[0083] pass Figure 2 Phase analysis shows that the diffraction peaks of the manganese tetraoxide prepared by the present invention are consistent with those of the standard substance, and do not show diffraction peaks of other substances, which further indicates that the manganese tetraoxide prepared by the present invention is a high-purity manganese tetraoxide product. Figure 3 It can be seen that the microscopic morphology of the manganese tetraoxide prepared by the present invention is regular spherical particles, and the particle size distribution is uniform. Figure 4 It can be seen that the apparent density of the agglomerate increases with the increase of the molding pressure. When the molding pressure increases to a certain level, the apparent density of the agglomerate gradually tends to be stable. Figure 5 Comparative analysis shows that compaction and calcination can effectively improve the tap density of manganese tetraoxide. In addition, adding a binder during the compaction molding process can also help improve the density of the molded agglomerates, thereby improving the tap density of manganese tetraoxide to a certain extent.

[0084] In summary, the present invention adopts manganese sulfate precipitation-compacting roasting method to prepare spherical, high-purity, high-tapped density manganese tetraoxide, by compacting the dried precipitation, and adding a binder in the molding process, adjusting the compactness of the agglomerate before oxidation roasting, and then realizing the regulation of oxygen kinetic transfer during oxidation roasting, effectively improving the tap density of the manganese tetraoxide product, the obtained manganese tetraoxide product has a regular morphology, uniform particle size distribution, high purity and tap density, and all indicators meet the industry standards of battery-grade manganese tetraoxide. Compared with direct roasting or other conventional strengthening methods, the manganese tetraoxide product prepared by the present invention increases with the increase of pressure applied by the briquetting, and the tap density will show a trend of first rising and then falling, especially at 40-50Mpa.

[0085] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing battery-grade high-purity, high-tap density manganese tetraoxide from a manganese sulfate solution, characterized in that: The steps include: S1: adding a surfactant to the manganese sulfate solution, heating, continuously stirring and slowly adding ammonia water to perform a precipitation reaction, and after the reaction is completed and cooled to room temperature, performing solid-liquid separation to obtain a precipitate; S2: washing the precipitate with deionized water and drying; S3: adding a certain amount of binder to the dried precipitate, and applying pressure to compact and shape it to obtain a molding material; S4: calcining the molding material, cooling, crushing and screening to obtain the trimanganese tetraoxide product.

2. The method for preparing battery-grade high-purity, high-tap density trimanganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S1, the concentration of the sulfuric acid solution is 0.2-1.5 mol / L; the concentration of the ammonia water is 10%-15%; and the surfactant is hexadecyltrimethylammonium bromide with a concentration of 0.5-5.0 g / L.

3. The method for preparing battery-grade high-purity, high-tap density trimanganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S1, the heating temperature is 50-80°C; the stirring rate is 300-500 r / min; the ammonia water addition time is 6-10 hours; and after the ammonia water is completely added, the reaction is continued for 4-12 hours.

4. The method for preparing battery-grade high-purity, high-tap density trimanganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S2, the drying temperature is 40 to 80°C, and the drying time is 8 to 15 hours.

5. The method for preparing battery-grade high-purity, high-tap density trimanganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S3, the binder is carboxymethyl cellulose, polyacrylamide or starch.

6. The method for preparing battery-grade high-purity, high-tap density manganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S3, the pressure is 5 to 100 MPa.

7. The method for preparing battery-grade high-purity, high-tap density trimanganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S3, the molding material is in the form of lumps or particles.

8. The method for preparing battery-grade high-purity, high-tap density trimanganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S4, the calcination temperature is 900-1150° C., and the calcination time is 1-4 hours.

9. The method for preparing battery-grade high-purity, high-tap density trimanganese tetraoxide from a manganese sulfate solution according to claim 1, characterized in that: In step S4, the tap density of manganese tetraoxide is as high as 2.88 g / cm 3 .

10. Use of manganese tetraoxide prepared by the method according to any one of claims 1 to 9 in batteries.

Citation Information

Patent Citations

  • Preparation method of manganese tetraoxide

    CN103011294A