Preparation process of advanced TFT-LCD (Thin Film Transistor-Liquid Crystal Display) glass substrate
Through multi-process collaborative innovation in the process flow, the floating process is optimized, and the problems of high control difficulty and many defects in the floating process are solved, and the preparation of high-quality, high mechanical strength and low defects are achieved. , ensuring the performance and stability of the glass substrate.
Patent Information
- Application Number
- CN202410965244.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
When preparing high-generation TFT-LCD glass substrates, existing float technology has problems such as many control parameters, high regulation difficulty and many microscopic defects, especially the contact surfaces between the glass liquid and the tin liquid are prone to microscopic tin points and scratches. Defects, it is difficult to stabilize the mechanical strength, thermal stability and surface defects of the glass substrate.
Through the optimization of the process flow, including combination innovations including ingredients, melting, clarification and homogenization, forming, annealing and grinding, the feeding system, electric melting and full oxygen are adopted, which combines specific raw material ratios, air nozzle blowing and air hammer vibration, and air fusion and full oxygen. Combustion heating method, multi-platinum channel clarification homogenization, grid heating and micro-edge puller forming technology, three-dimensional annealing kiln and efficient grinding process to achieve multi-process coordinated control of glass substrates, reducing bubbles, tin points and Scratch and other defects.
Effectively reduce or eliminate defects in glass substrates, improve quality, and achieve high-quality glass substrates with high mechanical strength, low heat shrinkage and few surface defects, ensuring excellent performance of glass substrates and stable industrial mass production.
Smart Images

Figure CN118908565A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of glass substrate manufacturing, and in particular to a float process for preparing a high-generation TFT-LCD glass substrate. Background Art
[0002] The electronic information display industry is an important pillar industry of my country's national economy. China is the world's largest producer of liquid crystal panels, accounting for 70% of the world's total production capacity. High-generation TFT-LCD glass substrates are the core materials and key strategic materials of the electronic information display industry and the pan-semiconductor industry. my country's annual demand for high-generation TFT-LCD glass substrates exceeds 300 million square meters.
[0003] The quality and performance of high-generation TFT-LCD glass substrates have a crucial impact on the display panel resolution, light transmittance, refresh rate, viewing angle and other qualities. Therefore, there are extremely high requirements for the quality of the substrate's interior and surface. Bubbles, stones, tin sticking, dripping and scratches are strictly controlled indicators in the glass substrate manufacturing process. Therefore, the production technology of high-generation TFT-LCD glass substrates is complex, and the production control accuracy is comparable to that of the semiconductor industry, representing the highest level in the field of modern glass scale manufacturing in the world.
[0004] There are two main molding processes for high-generation TFT-LCD glass substrates: float and overflow. The float molding process has the advantages of wide molding plates and low production costs, but it also has problems such as large mutual influence between multiple processes, many control parameters, high difficulty in regulation, and difficult to stably control the production status. In addition, in the float molding process, the glass liquid is thinned and formed on the surface of the metal tin liquid. The contact surface between the glass liquid and the tin liquid surface will have microscopic defects such as tiny tin spots and scratches. This contact surface is also the processing process surface of downstream LCD panel manufacturers. How to prepare micro-defect, high-quality, high-generation TFT-LCD glass substrates with excellent mechanical strength, thermal stability, thermal shrinkage and other properties, and few surface and internal defects through the float process is an important technical problem that needs to be solved urgently. Summary of the invention
[0005] In order to solve the technical problems existing in the prior art, the applicant's scientific researchers have made technical innovations in multiple processes of the display glass substrate production process through long-term, large-team, collaborative cooperation, and unremitting efforts, and have explored and utilized the advantages of each process, conducted combined innovation research between processes, and finally achieved a breakthrough in the float process of high-generation TFT-LCD glass substrates, forming a display glass substrate production process with full resource utilization, synergistic and complementary advantages, and organically unified production lines. This process can be used to prepare high-generation TFT-LCD glass substrates with relatively excellent control indicators and performance indicators such as bubbles, stones, tin adhesion, drips, and scratches, effectively reducing or eliminating defects in glass substrates, greatly improving the quality of glass substrates, and providing solutions for the preparation of micro-defect, high-quality, and high-generation display glass substrates.
[0006] The invention provides a glass substrate preparation process, which comprises the steps of batching, melting, clarifying and homogenizing, forming, annealing, grinding, cleaning, packaging and the like.
[0007] In the batching process, for the raw material composition, it is preferred to select SiO2, Al2O3, B2O3, MgO, CaO, SrO, ZrO2, and P2O5 batch materials that meet a specific ratio relationship, which can effectively reduce the boron volatilization rate during the glass forming process and eliminate the problem of uneven composition caused by boron volatilization. The aluminosilicate glass substrate prepared by using it has the characteristics of high strain point, high Young's modulus, high hardness, suitable thermal expansion coefficient, low thermal shrinkage rate, low defects, etc., which meets the special requirements of high-generation TFT-LCD glass substrates.
[0008] For the raw material batching method, it is preferred to use an electronic scale feeding system that combines air nozzle blowing and air hammer vibration. After the electronic scale bucket has weighed various raw materials, the materials are fed. While the pneumatic feeding valve is opened, the air nozzle blows the inner wall of the electronic scale bucket, and the air hammer strikes and vibrates the electronic scale bucket, so that the raw materials retained on the inner wall of the electronic scale bucket are discharged synchronously, ensuring that the components of each batch of materials are constant during the batching process, thereby ensuring the quality stability of the glass substrate.
[0009] In the melting process, it is preferred to adopt a heating method combining electric melting and full oxygen combustion. Electric heating can be achieved by using molybdenum electrodes or tin oxide electrodes, which can be set on the wall and / or bottom of the melting furnace, and the burner can be set on the roof and / or breast wall of the melting furnace. Preferably, the melting furnace is provided with a bubbling device and a kiln sill to perform primary debubbling and clarification on the molten glass liquid, and to discharge bubbles with a diameter of more than 0.2 mm in the molten glass liquid. Through the above-mentioned arrangement, the raw materials in the melting furnace are promoted to heat up synchronously, and the glass liquid is fully and efficiently melted; the primary debubbling and clarification of the melting furnace can better promote the debubbling of bubbles with a diameter of more than 0.2 mm in the melting furnace section. After debubbling, the number of bubbles with a diameter of more than 0.2 mm in the molten glass liquid is ≤0.1 / kg. And through the subsequent platinum channel precision clarification to remove bubbles with a diameter of less than 0.2 mm, the glass substrate can be fully debubbled and clarified to obtain high-quality glass liquid.
[0010] In the clarification and homogenization process, it is preferred to use a platinum channel clarification composed of 2 or more high-temperature platinum channels and 1 low-temperature platinum channel, and use optimized stirring and turbulence methods for forced homogenization. Compared with a single platinum channel, the reduced diameter of the platinum channel reduces the temperature difference of the glass liquid on the same cross-section of the channel. The improved turbulence process improves the efficiency of homogenization and promotes the full uniformity of the temperature and composition of the glass liquid flow; the lowering of the glass liquid level reduces the floating distance of the bubbles, and cooperates with the optimized raw material formula to jointly improve the bubble removal efficiency of small bubbles. Through the special design of the above-mentioned clarification and homogenization process, the generation of defects such as bubbles and streaks on the glass plate is avoided, and bubbles in the glass liquid are efficiently removed. The number of bubbles with a diameter of ≥0.05mm in the molten glass liquid does not exceed 0.15 / kg.
[0011] In the forming process, it is preferred to set a gridded heating unit on the top of the tin bath, and set a plurality of micro-edge-pulling machines in the forming thinning area. The heating unit and the edge-pulling machine are controlled in coordination, and the lateral temperature difference of the tin bath is adjusted by adjusting the output power of each lateral heating unit, so as to achieve different viscosities in the lateral direction of the glass ribbon. Under the action of the precise adjustment of the thinning force by the optimized combination of multiple micro-edge-pulling machines, the traction force of the appropriate main drive is matched to jointly achieve the precise thinning of the high-generation liquid crystal glass plate under multiple forces. The thickness difference of the prepared high-generation TFT-LCD glass substrate is ≤0.015mm.
[0012] In the annealing process, it is preferred to adopt an annealing kiln structure with precise temperature control based on a three-dimensional grid, and utilize methods such as cooling with turbulence-free cooling ducts, transmission with low thermal conductivity ceramic rollers, partition isolation with curtains, and differentiated insulation design of the annealing kiln to avoid air flow turbulence, reduce temperature field fluctuations, and reduce the lateral temperature difference of the glass substrate. This meets the requirements of constant lateral temperature of large-size ultra-thin glass substrates and precise matching of the temperatures of each zone of the annealing kiln with the annealing curve of the substrate, thereby achieving perfect matching of the temperature field with the annealing curve and fully eliminating stress on the glass substrate.
[0013] In the grinding process, three types of grinding pads with hardness ratios of 90HD-100HD: 60HD-70HD: 35HD-40HD are used to grind and polish the glass substrate in sequence, and the ratio of the grinding surface at the non-edge to the width of the grinding groove is optimized. Chamfers are set around the grinding disk and at the position of the grinding pad farthest from the grinding disk, and the chamfer angle on the grinding disk is greater than or equal to the chamfer angle of the grinding pad. This improves the grinding quality, reduces grinding scratches, and improves the grinding effect.
[0014] The above-mentioned high-generation TFT-LCD glass substrate float production process has fine control over the preparation process and realizes the organic synergy of various production process links. Through this process, the industrialized stable mass production of micro-defect, high-quality, high-generation float glass substrates for electronic applications has been realized first.
[0015] Beneficial effects of the present invention: The present invention fully explores and utilizes the advantages of multiple processes in the high-generation TFT-LCD glass substrate float production process, conducts combined innovation research between the processes, and forms a display glass substrate production process with an organically unified production line, outstanding advantages, and synergistic complementarity. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the overall process of glass substrate preparation process;
[0017] Figure 2 This is a schematic diagram of the feeding system for the batching process;
[0018] Figure 3 It is a schematic diagram of the front view and section of the melting furnace of the glass raw material melting process;
[0019] Figure 4 A schematic top view of a clarification and homogenization system for the clarification and homogenization process;
[0020] Figure 5 It is a schematic diagram of the transverse section of the tin bath in the forming process;
[0021] Figure 6 It is a top view schematic diagram of the tin bath forming thinning area in the forming process;
[0022] Figure 7 This is a top view of the annealing furnace for the annealing process;
[0023] Figure 8 This is a schematic diagram of the front cross section of the annealing furnace for the annealing process;
[0024] Fig. 9 Schematic diagram of the grinding process;
[0025] Fig.10 This is a schematic diagram of the surface of a glass substrate before and after grinding in the grinding process;
[0026] Fig.11 It is a schematic diagram of the structure of the polishing pad in the polishing process;
[0027] Fig.12 A schematic diagram of the grinding surface during the grinding process;
[0028] Fig.13 It is a schematic diagram of the structure of the grinding device for the grinding process;
[0029] Fig.14 for Fig.13 Enlarged view of point A in the middle;
[0030] Fig.15 This is a schematic diagram of the chamfering of the grinding disc during the grinding process;
[0031] Fig.16 Schematic diagram of the chamfering of the grinding pad during the grinding process. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the protection scope of the present application. It is understood that the drawings are only provided for reference and explanation, and are not used to limit the present application.
[0033] Specifically, the present application embodiment provides a high-generation TFT-LCD glass substrate float process, such as Figure 1 As shown, the glass substrate preparation process mainly includes the following processes:
[0034] Batching process: select appropriate raw material composition, weigh and mix the raw materials to form glass batch;
[0035] Melting process: heating and melting the uniformly mixed glass batch materials to form molten glass liquid;
[0036] Clarification and homogenization process: The molten glass is passed through a clarification channel to remove bubbles and homogenize;
[0037] Forming process: flatten and thin the molten glass on the surface of the metal tin liquid to form a glass substrate;
[0038] Annealing process: annealing the glass substrate to eliminate the internal stress in the glass substrate;
[0039] Grinding process: cutting the glass substrate to the required size and grinding it;
[0040] Cleaning process: cleaning the glass substrate;
[0041] Packaging process: Packaging the cleaned and tested qualified glass substrates.
[0042] Below, each process technology is explained one by one.
[0043] Batching process:
[0044] High-generation TFT-LCD glass substrates require the following characteristics: low density, high strain point, appropriate thermal expansion coefficient, high Young's modulus, chemical corrosion resistance, low thermal shrinkage, and low micro defects. To this end, the raw material components need to be carefully designed.
[0045] Preferably, the following materials are used in weight fraction ratio: 60-72% SiO2, 13-18% Al2O3, 8.5-10% B2O3, 1-4.5% MgO, 3-8% CaO, 1-5% SrO, 0.5-2% ZrO2, 1-5% P2O5, 0.1-0.5% SnO2; wherein SiO2+Al2O3 is 76-85%; (MgO+CaO+SrO) / Al2O3 is 0.4-0.7%; the total amount of alkaline earth metal oxides is 5-11.5%; B2O3 / (B2O3+ZrO2+P2O5) is 0.6-0.9%; (ZrO2+P2O5) / (MgO+CaO+SrO) is 0.15-0.8%.
[0046] The above-mentioned glass material can effectively reduce the boron volatilization rate during the glass forming process, control the uneven glass liquid composition caused by boron volatilization during the preparation of the glass substrate, and in addition, the raw material can also promote the degassing and clarification of the glass liquid. The aluminosilicate glass substrate prepared using the raw material has the characteristics of high strain point, high Young's modulus, high hardness, appropriate thermal expansion coefficient, low thermal shrinkage, low micro-defects, etc., among which the β-OH value is less than 0.5%, the boron volatilization rate is less than 11%, and the thermal expansion coefficient in the range of 50-350℃ is less than 39.5×10 -7 / ℃, Young's modulus is higher than 78GPa, strain point is higher than 690℃, melting temperature is lower than 1690℃, and thermal shrinkage is lower than 11.5ppm.
[0047] At the same time, the quality requirements of high-generation TFT-LCD glass substrates are much higher than other types of glass. This requires that the components of high-generation TFT-LCD glass substrate ingredients maintain very high uniformity and no obvious differences in components can occur. This places strict requirements on the purity, weighing accuracy, and mixing uniformity of various raw materials in the ingredients.
[0048] Preferably, the following electronic weighing system for controlling the stability of the glass batch composition can be used.
[0049] like Figure 2As shown, the system includes an electronic weighing bucket 101, a pneumatic feeding valve 102 is provided at the bottom of the electronic weighing bucket, an air hammer 103 is provided on the outer wall of the electronic weighing bucket 101, the pneumatic feeding valve 102 is opened and closed by an opening solenoid valve 104 and a closing solenoid valve 105 respectively, the opening solenoid valve 104 is also connected to the air hammer 103, the opening solenoid valve 104 is connected to a first air pipe 106 and a second air pipe 107, the first air pipe 106 is connected to the pneumatic feeding valve 102, and the second air pipe 107 is connected to the air hammer 103; the closing solenoid valve 105 is provided with a third air pipe 108, and the third air pipe 108 is connected to the pneumatic feeding valve 102; an air nozzle 109 is provided on the upper part of the inner wall of the electronic weighing bucket 101, the air nozzle 109 is connected to a fourth air pipe 110 extending out of the electronic weighing bucket 101, and the fourth air pipe 110 is communicated with the first air pipe 106. The air nozzle 109 can be set at a place where materials are often easily accumulated according to actual needs. If there are multiple places where materials are accumulated, multiple air nozzles 109 are set accordingly. Through the above system, the various components in the glass raw material batching can be stably proportioned. Specifically, when the electronic scale bucket 101 weighs various glass raw materials and then feeds them, while the pneumatic feeding valve 102 is opened, the air nozzle 109 blows air to the inner wall of the electronic scale bucket 101, and the air hammer 103 hits the electronic scale bucket 101, so that the raw materials retained on the inner wall of the electronic scale bucket 101 are discharged synchronously, thereby ensuring the stability of the components of each batch material in the liquid crystal glass batching process and ensuring the quality of the glass substrate.
[0050] The above-mentioned batching process is adopted to improve the quality and performance of the glass substrate from the source, and ensure the accuracy and stability of the batching.
[0051] Melting process:
[0052] After the above batching process is completed, the glass raw materials are melted through a melting process.
[0053] Preferably, the following melting process may be adopted.
[0054] like Figure 3As shown, electrodes 202 are symmetrically or staggeredly arranged on the inner wall and / or the bottom of the pool on both sides of the melting furnace 201, and all-oxygen burners 203 are arranged on the roof and / or the breast wall of the melting furnace 201. When arranged on the roof, the all-oxygen burners are vertically distributed, the flame jets are vertically downward, and the flame can contact the liquid surface of the glass liquid in the melting furnace 201. When arranged on the breast wall, the all-oxygen burners are arranged horizontally. The glass raw materials are completely melted by direct heating of the electrodes and radiation heating of all-oxygen combustion. The melting furnace is preferably also provided with a bubbling device 204 and a kiln sill 205 to perform primary bubble removal and clarification on the molten glass liquid, so as to discharge larger bubbles in the glass liquid. Through the careful combination of raw materials, the use of a full-dimensional three-dimensional electric-gas all-oxygen combustion composite heating method, and the effects of bubbling and kiln sills, the number of bubbles with a bubble diameter of more than 0.2 mm in the molten glass liquid is greatly reduced, and the number of bubbles with a bubble diameter of more than 0.2 mm is ≤0.1 / kg.
[0055] By adopting the above process, the glass raw materials are heated from multiple angles from bottom to top, and the raw materials at each position in the melting furnace are heated evenly and fully. At the same time, the special selection of glass raw materials promotes the coordinated cooperation of the primary clarification and the precise clarification of the glass liquid in the primary clarification and clarification homogenization sections of the melting furnace, thereby improving the defoaming efficiency of the production line system and the quality of the glass substrate.
[0056] Clarification and homogenization process:
[0057] The melted glass raw materials become molten glass, which needs to go through a clarification and homogenization process before being molded.
[0058] Preferably, the following process can be used for clarification and homogenization.
[0059] like Figure 4As shown, the platinum channel includes a plurality of high-temperature platinum channels and a low-temperature platinum channel (a stirring section after confluence, a second cooling section, and a feeding section). The first high-temperature platinum channel (310) is composed of a first inlet section (311), a first clarification section (312), a first cooling section A (313), and a first stirring section (314) connected in sequence, and the second high-temperature platinum channel (320) is composed of a second inlet section (321), a second clarification section (322), a first cooling section B (323), and a second stirring section (324) connected in sequence, the ports of the first inlet section (311) and the second inlet section (321) are connected to the melting furnace (201), the ports of the first stirring section (314) and the second stirring section (324) are both connected to the stirring section (340) after confluence, and the stirring section (340) after confluence is also connected in sequence to the second high-temperature platinum channel (320). A low-temperature platinum channel is composed of a cooling section (350) and a feeding section (360), wherein the feeding section (360) is connected to a tin bath; the first cooling section A (313) and the first cooling section B (323) are used to cool the glass liquid flowing therethrough and control the cooling rate to achieve the process temperature required by the stirring section; the second cooling section (350) is also used to cool the glass liquid flowing therethrough and, when necessary, to heat the glass liquid flowing therethrough to meet the glass forming requirements; grilles with different installation angles are sequentially arranged from right to left inside the second cooling section (350), and the installation angles of adjacent grilles are different, so that the holes on the grilles are staggered to ensure that the glass liquid forms a turbulent flow after passing through the grilles.
[0060] The above-mentioned multi-platinum channel clarification and homogenization process reduces the heat load of a single platinum channel and avoids the risk of collapse of a large-diameter platinum channel due to long-term high-temperature operation; the platinum channel with a reduced diameter reduces the temperature difference between the center temperature of the glass liquid and the contact part of the platinum body on the same cross-section of the channel, and the improved stirring and grid turbulence process improves the efficiency of homogenization and the homogeneity of the glass liquid. Through this homogenization process, the temperature and composition of the glass liquid can be fully uniform, and the quality of the glass substrate can be improved. Due to the reduction of the glass liquid level, the bubble removal efficiency of small bubbles is improved, and the number of bubbles with a diameter of ≥0.05mm in the molten glass liquid does not exceed 0.15 / kg. The coordinated cooperation of raw material selection, primary clarification of the melting furnace, and precision clarification and homogenization can remove bubbles from the glass liquid with high quality.
[0061] Molding process:
[0062] After completing the above-mentioned clarification and homogenization process, the glass liquid is subjected to float thinning and forming.
[0063] Preferably, the following process can be used for float thinning.
[0064] like Figure 5 , Figure 6As shown, the molten glass flows into the forming tin bath. The tin bath is divided into a bath pool 401, a breast wall 402 and a top cover 403 from bottom to top; along the flow direction of the glass liquid, the tin bath is divided into a forming and drawing area 404, a shaping and cooling area and a temperature homogenization area.
[0065] The top of the tin bath is divided into a grid of multiple heating units 405 with the glass liquid flow direction as the longitudinal direction and perpendicular to the glass liquid flow direction as the transverse direction, and each heating unit can independently control the heating temperature. Each heating unit includes one or more heating elements. The TFT-LCD glass substrate has the characteristics of high molding temperature and volatile components. For this reason, the heating element is preferably a high-density three-phase silicon carbon rod.
[0066] It is preferred to increase the density of the gridded heating units in the forming and thinning area, so as to more finely control the temperature of each area and improve the accuracy and flexibility of temperature control.
[0067] In conjunction with the tin bath heating system, it is preferred to use a precision thinning system in the forming and thinning area for coordinated control. The TFT-LCD glass liquid has a short material property and a small forming temperature range, so the spacing between the edge stretchers is reduced, the number of edge stretchers is increased, and within a limited temperature range, the action range of the thinning system is reduced, and the glass strip thinning force can be subdivided to each pair of edge stretchers to achieve ultra-thin precision forming of the glass substrate. The precision thinning system uses a micro edge stretcher 406, the edge stretcher body is less than 300mm, preferably 200-250mm; the distance between two adjacent edge stretchers is less than 1000mm, preferably 500-900mm. A total of 15-25 pairs of edge stretchers are set in the forming and thinning area, preferably 18-22 pairs.
[0068] Preferably, at least part of the lateral edge heating units 415 are arranged corresponding to the edge drawing machines, and one edge heating unit corresponds to 1 to 4 edge drawing machines, preferably 2 to 3.
[0069] The control system uniformly adjusts each heating unit and the edge drawing machine. By adjusting the output power of each heating unit in the horizontal direction, the lateral temperature difference of the tin bath is adjusted, thereby adjusting the viscosity difference of the glass ribbon in the horizontal direction. The thinning force of the edge drawing machine acts on the edge of the glass ribbon and is transmitted to the middle of the glass ribbon. The influence of the lateral temperature difference of the tin bath on the viscosity of the glass liquid is coupled with the regulation of the thinning force of the edge drawing machine, thereby improving the lateral thinning effect of the glass ribbon and achieving a thickness difference of ≤0.015mm for the entire high-generation TFT-LCD glass substrate.
[0070] Annealing process:
[0071] After the above float glass forming is completed, the formed glass substrate needs to be annealed.
[0072] Preferably, the following glass annealing process may be adopted.
[0073] like Figure 7 , Figure 8As shown, a grid control method is adopted in the annealing process to divide the annealing area into multiple partitions 501, and each partition 501 can be independently temperature controlled. Each partition includes a temperature detection device 502, a heating device 503 and a cooling device 504. The cooling device adopts a cooling air duct, the air inlet is outside the kiln body, and a centrifugal fan 505 is provided at the air outlet. The air flows in the cooling air duct to reduce the temperature of the cooling air duct. The cooling air duct reduces the temperature of each partition, and this method avoids air disturbance.
[0074] The applicant has found that one of the reasons for the poor mechanical properties of the liquid crystal glass substrate is that the same glass substrate has large internal stress in the lateral direction. The reason is that the lateral annealing temperature is inconsistent. Since the temperature of the lateral edge of the glass substrate is lower than the temperature of the middle, if the temperature is not controlled differently, it is easy to cause different lateral annealing temperatures, resulting in large internal stress. Therefore, it is preferred that at least in part of the annealing area, the temperature of the subarea 506 corresponding to the glass edge is higher than the temperature of the subarea 507 corresponding to the glass center.
[0075] It is preferred to use a ceramic roller as the transmission roller 508. The ceramic roller has excellent heat insulation effect and can prevent heat conduction between the glass substrate and the ceramic roller to the greatest extent, thereby avoiding unexpected cooling of the glass substrate. A curtain 509 is provided in the annealing furnace, and the curtain can be raised and lowered under control. Unlike other float glasses, the ultra-thin glass is transported at a faster speed in the annealing furnace. During the transportation process, airflow is easily formed. The use of the curtain avoids the flow of airflow, which is more conducive to the independence and precise temperature control of each zone.
[0076] It is further preferred that the temperature of the annealing furnace insulation layer is different from the inside to the outside, with the temperature inside being high and the temperature outside being low. By setting insulation materials with different thermal conductivity in the heat transfer direction of the insulation layer, the inner high temperature layer 510 uses insulation materials with lower thermal conductivity to reduce the overall thermal conductivity. Furthermore, the thermal bridges such as the connecting plates and plug holes between the inner and outer walls of the annealing furnace are connected by thermal break bridges to further reduce heat conduction, and the temperature difference between the outer wall and the environment is reduced to less than 2 / 3 of the original temperature difference between the outer wall and the environment. Through the above means, temperature fluctuations caused by frequent temperature adjustment can be avoided, and the temperature stability in the annealing furnace can be improved.
[0077] The temperature detection device, heating device, cooling device, and curtain lifting device of each partition are all connected to the control device, and automatic intelligent control of the above devices is achieved through the control device.
[0078] The annealing process of the present invention can better meet the requirements for precise matching of the temperature field and annealing curve of a high-generation TFT-LCD glass substrate, reduce the lateral temperature difference of the glass substrate, avoid temperature field fluctuation and disorder, effectively eliminate the internal stress of the glass substrate, and realize differentiated, refined, automated and intelligent control of annealing.
[0079] Grinding process:
[0080] After the glass is annealed, the glass substrate needs to be ground. Grinding refers to grinding the uneven parts of the glass surface and microscopic defects such as tin sticking and scratches. By adding abrasives, additives and other chemical components, the glass surface can be made smooth and flat to achieve the grinding effect.
[0081] Polishing is performed after initial grinding to further smooth the glass surface and improve its flatness.
[0082] like Fig. 9 As shown, the grinding process of this embodiment is mainly carried out in the following manner:
[0083] Clean and remove dust from the glass substrate;
[0084] The glass substrate is coarsely ground by using a coarse grinding pad and a grinding liquid;
[0085] Fine grinding the roughly ground glass substrate by using a fine grinding pad and a grinding liquid;
[0086] The finely ground glass substrate is polished by using a polishing pad and a polishing liquid;
[0087] The polished glass substrate is cleaned.
[0088] Among them, when the glass is not ground, the surface of the glass appears as follows Fig.10 As shown in the shape of ①, the glass surface presents many irregular shapes and structures, which will lead to reduced light transmittance of the glass and deformation of the image.
[0089] Before grinding, the glass needs to be cleaned and dusted.
[0090] During grinding, the coarse grinding pad provided on the grinding piece and the grinding liquid grind the glass substrate together, Fig.10 The shape of ① is ground to Fig.10 The shape of ② in the middle eliminates the uneven area of the glass substrate.
[0091] After the rough grinding is completed, the fine grinding pad set on the grinding piece and the grinding liquid grind the glass substrate together to remove the extremely fine scratches on the glass substrate. Fig.10 The shape of ② is ground to Fig.10 The form of ③.
[0092] After the fine grinding is completed, the polishing pad set on the grinding piece and the grinding liquid grind the glass substrate more deeply. After the polishing pad grinds the glass substrate, the defects on the glass substrate that are invisible to the naked eye can be polished away, and the glass substrate is Fig.10 The shape of ③ is ground to Fig.10The shape of ④ meets the high quality requirements of TFT-LCD glass substrates.
[0093] Grinding equipment to be used in the grinding process, such as Figure 11-Figure 14 As shown, the grinding device includes a grinding disc 620 and a grinding pad 610. The grinding pad 610 is assembled on the grinding disc 620. The side of the grinding pad 610 away from the grinding disc 620 grinds the glass. The grinding pads are composed of a grinding substrate 614 and a grinding particle layer 613. The hardness of the grinding particle layer 613 on different grinding pads 610 is different.
[0094] For the hardness range, the coarse grinding pad: fine grinding pad: polishing pad is preferably controlled to be 90HD-100HD: 60HD-70HD: 35HD-40HD, and further preferably 90HD-95HD: 60HD-70HD:
[0095] 35HD-40HD, and further preferably 90HD-95HD: 65HD-70HD: 35HD-40HD. In the above, HD is the Shore hardness index. Fig.11 and Fig.12 As shown, in order to improve the grinding effect, a grinding groove 611 is formed on the grinding pad 610, and multiple grinding grooves 611 are interconnected to facilitate the flow of grinding liquid. A plurality of grinding surfaces 612 are formed on the grinding pad 610, and preferably, except for the grinding surface at the edge, the other grinding surfaces are square, and the grinding surface 612 grinds the surface of the glass substrate.
[0096] The ratio of the width of the grinding surface at the non-edge to the width of the grinding groove is preferably 1:1-3:1, and more preferably 1.7:1-2.3:1.
[0097] In the embodiment of the present application, the matching relationship between the grinding pad 610 and the grinding disk 620 can also affect the grinding effect of the glass substrate. The main impact is that during the grinding process, the working surface of the edge of the grinding pad 610 and the processing surface of the glass substrate are not completely parallel.
[0098] In the existing technology, the edge of the grinding pad is basically perpendicular to the processing surface. In this structure, the edge of the grinding pad will scratch the glass substrate to a certain extent during the grinding process, and the scratch will cause wear marks on the glass.
[0099] After many simulations and studies, the applicant found that the specially designed double chamfer coupling can greatly reduce the probability of the polishing pad scratching the glass substrate during polishing. The specific method is as follows:
[0100] The grinding disc 620 is chamfered around the edges. In the embodiment of the present application, the chamfer is chamfered 621. The chamfering method is as follows: Fig.15Take the height of the side of the grinding disc as H, extend the bottom of the grinding disc vertically upward along the side for a distance h to point a, take the side of the grinding disc as one side, take point a as the vertex, make the other side with the round chamfer angle, the intersection of the other side and the bottom of the grinding disc as point b, connect points a and draw an isosceles triangle with this as one side, and the side length of the isosceles triangle is the radius R of the round chamfer. Among them, h / H = 1:2-1:6, preferably 1:3-1:5, and more preferably 1:3.5-1:5.
[0101] Preferably, the grinding pad is chamfered around the grinding disc 620 .
[0102] At the same time, Fig.13 and Fig.14 The edge of the grinding pad shown in the figure is far away from the grinding disc 620, that is, facing the glass substrate. There is also a chamfer, preferably a straight chamfer 615. The straight chamfer 615 can further prevent the glass substrate from being scratched on the basis of the round chamfer 621. Fig.16 The position of the straight chamfer is at position c on the side of the grinding pad, the distance between c and the bottom surface of the grinding pad is h', the thickness of the side of the grinding pad is H', h' / H'=4:5-1:2, preferably 4:5-3:5. As for the relationship between the chamfer angle of the grinding disc and the chamfer angle of the grinding pad, it is preferred that the chamfer angle of the grinding disc is greater than or equal to the chamfer angle of the grinding pad, it is further preferred that the chamfer angle of the grinding disc is greater than or equal to the chamfer angle of the grinding pad and the chamfer angle of the grinding disc is ≥50°, it is further preferred that the chamfer angle of the grinding disc is greater than or equal to the chamfer angle of the grinding pad and the chamfer angle of the grinding disc is ≥60°, it is further preferred that the chamfer angle of the grinding disc is greater than or equal to the chamfer angle of the grinding pad, and 75°≥the chamfer angle of the grinding disc is ≥60°.
[0103] Glass grinding liquid is a material that plays an important role in the glass manufacturing and processing process. The grinding liquid is mainly composed of abrasives, solvents and other additives. These components are suspended in the liquid in the form of particles. The main function of the glass grinding liquid is to remove impurities on the surface of the glass by grinding particles to achieve the purpose of smoothing the glass surface. The glass grinding liquid used in the present invention preferably includes cerium oxide, lanthanum oxide, fluoride, praseodymium oxide, silicon oxide, aluminum oxide, calcium oxide and iron oxide, with a concentration range of 1-10%.
[0104] In the embodiment of the present application, in order to improve the grinding effect, the grinding pressure, grinding temperature and grinding speed can be controlled.
[0105] The grinding pressure can be controlled between 0.01-0.3 MPa, preferably 0.01-0.28 MPa, more preferably 0.1-0.25 MPa, further preferably 0.1-0.2 MPa, most preferably 0.15-0.2 MPa.
[0106] The grinding temperature can be controlled within the range of 20-60°C, preferably 20-50°C, more preferably 30-50°C, and even more preferably 30-40°C.
[0107] The grinding speed can be controlled between 5000 rpm and 7000 rpm, preferably between 5200 rpm and 6500 rpm, more preferably between 5500 rpm and 6300 rpm, and further preferably between 5800 rpm and 6000 rpm.
[0108] The grinding time can be controlled between 30 seconds and 300 seconds, preferably between 60 seconds and 240 seconds, and more preferably between 80 seconds and 150 seconds.
[0109] Cleaning process:
[0110] After completing the above process, the glass substrate needs to be cleaned. The cleaning process is mainly to remove the residual grinding fluid and other impurities on the surface of the glass substrate, so as to facilitate the roughness test of the glass substrate using the Surtronic S-100 series surface roughness tester.
[0111] The glass substrate is deeply cleaned by disk brush, roller brush, ultrasound, two-fluid, etc. to achieve the purpose of cleaning the glass surface.
[0112] Packaging process:
[0113] After cleaning and inspection, qualified glass substrates are packaged to prevent the glass from being hit and causing cracks and gaps, which would affect the sale of the glass in the market.
[0114] Example:
[0115] The examples of this application focus on describing the grinding process of the present invention.
[0116] The grinding liquid in the embodiment is made of grinding powder with cerium oxide as the main component (cerium oxide content 58%) and 0.2 megohm (MΩ) pure water, with a concentration range of 4%. In the following grinding process, grinding is based on the composition of the glass grinding liquid. For the grinding disk, h / H=1:4, h=4mm, and for the grinding pad, h' / H'=3 / 4.
[0117] In the embodiment of the present application, the hardness range of the coarse grinding pad is between 90HD-100HD, the hardness range of the fine grinding pad is between 60HD-70HD, and the hardness range of the polishing pad is between 35HD-45HD. The combination of grinding pads 610 of different hardness can produce different effects of glass surface flatness.
[0118] In the embodiment of the present application, the grinding pressure is 0.15 MPa, the grinding temperature is 35° C., the grinding speed is 6000 rpm, and the grinding time is 140 seconds.
[0119] The roughness is tested by Surtronic S-100 series surface roughness tester.
[0120] The combined grinding effects of various grinding pads with different hardness are shown in Table 1 below:
[0121] Table 1:
[0122]
[0123]
[0124] Among them, flatness refers to the degree of deviation between the geometric shape of the glass substrate surface and the ideal plane, usually expressed by the distance between two points or the radius of curvature. The flatness of high-generation TFT-LCD glass substrates has a great influence on the strength, optical properties, physical properties, etc. of the glass substrate. Therefore, during the manufacturing process, the flatness needs to be strictly controlled and tested; the glass scratch defect rate mainly refers to the probability that the surface molding and processing scratches of the semi-finished glass substrate are not completely eliminated after grinding. The lower the glass scratch defect rate, the fewer scratches remain on the glass surface after grinding.
[0125] From Table 1 above, we can see that when the coarse grinding pad: fine grinding pad: polishing pad are selected from 90HD-100HD: 60HD-70HD: 35HD-40HD, they can have good performance in terms of flatness compliance rate and scratch defect rate after grinding. When 90HD-95HD: 65HD-70HD: 35HD-40HD are selected, they can have better performance in terms of flatness compliance rate and scratch defect rate after grinding.
[0126] In the embodiment of the present application, the ratio of the non-edge grinding surface 612 to the width of the grinding groove 611 is set to a ratio of 1:1-3:1. The grinding pads that meet this ratio can complete the grinding of the glass substrate well. The applicant has found through a lot of experiments and research that:
[0127] Compared with the optimal solution, when the ratio of the width of the non-edge grinding surface 612 to the grinding groove 611 is 1:1-1.7:1, the flow guiding effect is good and the grinding liquid flow rate is fast, but the grinding contact area is small and the grinding efficiency is relatively low;
[0128] When the width ratio of the non-edge grinding surface 612 to the grinding groove 611 is 1.7:1-2.3:1, the flow guiding effect of the grinding liquid and the grinding efficiency are taken into consideration, and secondary defects are not easily generated while ensuring the grinding efficiency;
[0129] Compared with the optimal solution, when the ratio of the width of the non-edge grinding surface 612 to the grinding groove 611 is 2.3:1-3:1, the grinding efficiency is high, but the flow guidance effect is poor, the fluidity of the grinding liquid is poor, and secondary defects are more likely to occur.
[0130] Therefore, according to the test results, when the ratio of the width of the non-edge grinding surface 612 to the grinding groove 611 is 1.7:1-2.3:1, Fig.12 As shown in Figure ②, the flow guidance effect of the grinding liquid and the grinding efficiency are taken into consideration, which can better meet the needs of high-quality glass substrate manufacturing.
[0131] For the selection of round chamfer and straight chamfer, the occurrence rate of wear marks on the glass caused by different angles is shown in Table 2:
[0132] Table 2:
[0133]
[0134]
[0135] According to the data in the above table, when the chamfer angle of the grinding disc is greater than or equal to the chamfer angle of the grinding pad, and the chamfer angle of the grinding disc is ≥60°, the occurrence rate of wear marks is low and a better grinding effect can be achieved.
[0136] The above embodiments are only used to illustrate the technical method of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical method of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical method of the present invention.
Claims
1. A float process for preparing a high-generation TFT-LCD glass substrate, characterized in that: The process is composed of multiple process systems, including: Batching process: select the raw material formula of alkali-free aluminoborosilicate glass, weigh and mix various raw materials, and feed them into the melting furnace. When feeding, adopt the blowing or vibration method to prevent material stagnation or accumulation; Melting process: The glass batch is melted into molten glass liquid by using electrode fluxing and full oxygen combustion composite heating method; Clarification and homogenization process: a platinum channel composed of multiple high-temperature platinum channels and one low-temperature platinum channel clarifies and homogenizes the molten glass; Forming process: The molten glass floats on the surface of the tin liquid to form a continuous glass ribbon. The independently temperature-controlled heating unit in the tin bath and the thinning force of the micro-edge-pulling machine are regulated to thin the glass ribbon into a glass substrate. Annealing process: The annealing furnace is divided into multiple zones, each with independent temperature control, to anneal the glass substrate; Grinding process: The glass substrate is ground and polished in sequence using three grinding pads of coarse grinding, fine grinding and polishing with a hardness ratio of 90HD-100HD: 60HD-70HD: 35HD-40HD in combination with a grinding liquid.
2. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 1, characterized in that: In the batching process, the raw material formula is 60-72% SiO2, 13-18% Al2O3, 8.5-10% B2O3, 1-4.5% MgO, 3-8% CaO, 1-5% SrO, 0.5-2% ZrO2, 1-5% P2O5, 0.1-0.5% SnO2, wherein SiO2+Al2O3 is 76-85%, (MgO+CaO+SrO) / Al2O3 is 0.4-0.7%, and alkaline earth metal oxide is 0. The total amount of materials is 5-11.5%, B2O3 / (B2O3+ZrO2+P2O5) is 0.6-0.9%, (ZrO2+P2O5) / (MgO+CaO+SrO) is 0.15-0.8%, and the boron volatility of the raw material composition is lower than 11%; the raw materials are weighed according to the above raw material formula, and when feeding, the materials retained on the inner wall of the weighing bucket are discharged synchronously through the blowing of the air nozzle arranged on the inner wall of the weighing bucket and the vibration of the air hammer arranged on the outer wall of the weighing bucket, and a plurality of air nozzles can be arranged according to the material accumulation situation.
3. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 1, characterized in that: In the melting process, the raw materials are heated and melted by electrodes installed on the inner walls on both sides of the melting furnace and / or the bottom of the pool, and the full oxygen burner installed on the top and / or breast wall of the melting furnace. A bubbling device and a kiln sill are installed in the melting furnace.
4. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 1, characterized in that: The low-temperature section platinum channel includes a stirring device and multiple grids. The installation angles of adjacent grids are different, so that the holes on adjacent grids are misaligned. The stirring of the stirring device and the turbulence of the multiple grids achieve full homogenization of the molten glass.
5. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 1, characterized in that: In the forming process, the lateral temperature difference of the tin bath is adjusted by controlling the output power of each lateral heating unit, and the thinning force of the micro-edge stretching machine set at the same lateral position of the above-mentioned heating unit is coordinated to be adjusted, so that the glass ribbon is thinned and formed.
6. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 1, characterized in that: In the annealing process, the glass substrate is transported by a ceramic roller as a transmission roller. In at least part of the annealing area in the annealing furnace, the temperature of the partition corresponding to the edge of the glass substrate is higher than the temperature of the partition corresponding to the center of the glass substrate. The thermal conductivity of the high-temperature layer insulation material on the inner side of at least part of the kiln wall is lower than the thermal conductivity of the low-temperature layer insulation material on the outer side.
7. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 1, characterized in that: In the grinding process, the hardness of the coarse grinding pad, the fine grinding pad and the polishing grinding pad is selected to be 90HD-95HD: 60HD-70HD: 35HD-40HD.
8. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 7, characterized in that: In the grinding process, the hardness of the coarse grinding pad, the fine grinding pad and the polishing grinding pad is selected to be 90HD-95HD: 65HD-70HD: 35HD-40HD.
9. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 7, characterized in that: The polishing pad includes a plurality of polishing surfaces divided by polishing grooves. Except for the polishing surface at the edge, the other polishing surfaces are square. The ratio of the width of the polishing surface at the non-edge to the width of the polishing groove is 1:1-3:
1.
10. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 9, characterized in that: The grinding pad is assembled on the grinding disc, and the grinding disc forms chamfers on the sides of one side facing the grinding pad, and the grinding pad is closely attached to the grinding disc, and the grinding pad forms chamfers on the sides of the side away from the grinding disc.
11. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 10, characterized in that: The grinding disc forms a round chamfer in the surrounding direction of the side facing the grinding pad, and the grinding pad forms a straight chamfer in the surrounding direction of the side away from the grinding disc.
12. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 11, characterized in that: The chamfer angle of the grinding pad is ≤ the chamfer angle of the grinding disc.
13. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 12, characterized in that: The chamfer angle of the grinding disc is ≥ the chamfer angle of the grinding pad, and the chamfer angle of the grinding disc is ≥60°.
14. The float process for preparing a high-generation TFT-LCD glass substrate according to claim 13, characterized in that: The chamfer angle of the grinding disc is ≥ the chamfer angle of the grinding pad, and 60°≤the chamfer angle of the grinding disc≤75°.
Citation Information
Patent Citations
Grinding and polishing method for TFT-LCD glass base plate
CN109909869A
Grinding disc and chemical mechanical grinding device
CN110450046A
Alkali-free aluminoborosilicate glass
CN111606560A
High-generation TFT-LCD float glass substrate processing line
CN115196866A
High-generation display glass production process
CN117164214A
Cited By
TFT (Thin Film Transistor) alkali-free glass substrate capable of inhibiting microcrack propagation and having high interface bonding energy and preparation method of TFT alkali-free glass substrate
CN120172640A