Optical glass, preform and optical element

By rationally preparing components such as P2O5, Nb2O5, Na2O, K2O, etc. in optical glass, the problem of changes in imaging characteristics of optical glass in high temperature environments is solved, and the correction and cost reduction of imaging characteristics by temperature changes is achieved, while improving the bondability of glass and transmittance.

CN118908566APending Publication Date: 2024-11-08OHARA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964910.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-02-28
Filing Date
2018-04-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The temperature changes of existing optical glasses under high temperature environments have negative effects on imaging characteristics, and lack glasses with negative relative refractive index temperature coefficient and small absolute value, as well as glass materials with large average linear thermal expansion coefficient.

Method used

Through glass containing components such as P2O5, Nb2O5, Na2O, K2O, etc., the relative refractive index temperature coefficient is controlled within the range of +3.0×10-6 to -10.0×10-6°C-1, and the average linear thermal expansion coefficient is increased to 80 (10) -7°C-1 or above, to realize correction of the impact on imaging characteristics.

Benefits of technology

Effective correction of the impact on imaging characteristics under high temperature environments is achieved, the production cost of optical glass is reduced, and the engagement and visible light transmittance with low refractive index and low dispersion glass materials are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004951463250000131
    Figure BDA0004951463250000131
  • Figure BDA0004951463250000141
    Figure BDA0004951463250000141
  • Figure BDA0004951463250000151
    Figure BDA0004951463250000151
Patent Text Reader

Abstract

The invention provides optical glass which is low in temperature coefficient value of relative refractive index and contributes to correction of influence of temperature change on imaging characteristics, and a preformed body and an optical element using the optical glass. The optical glass contains, in mass%, 20.0% to 40.0% of a P2O5 component and 25.0% to 50.0% of a Nb2O5 component, the mass sum (Na2O + K2O) is 3.0% to 30.0%, and the temperature coefficient of the relative refractive index of 589.29 nm at 40 DEG C to 60 DEG C is in the range of + 3.0 * 10 <-6 > (DEG C <-1 >) to-10.0 * 10 <-6 > (DEG C <-1 >).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical glass, a preform and an optical element. Background Art

[0002] In recent years, the use of optical components in vehicle-mounted optical devices such as vehicle-mounted cameras, or in optical devices that generate a lot of heat, such as projectors, copiers, laser printers, and playback devices, has continued to increase in high-temperature environments. In such high-temperature environments, the temperature of the optical components that constitute the optical system is prone to large changes during use, and it is common for the temperature to reach more than 100°C. At this time, the negative impact of temperature changes on the imaging characteristics of the optical system has become so large that it cannot be ignored. Therefore, it is necessary to construct an optical system that is unlikely to affect the imaging characteristics even if the temperature changes.

[0003] When constructing an optical system in which imaging characteristics are less likely to be affected by temperature changes, it is preferred to use an optical element composed of glass whose refractive index decreases when the temperature rises and whose relative temperature coefficient of refractive index is negative, and an optical element composed of glass whose refractive index increases when the temperature rises and whose relative temperature coefficient of refractive index is positive. This can correct the effects of temperature changes on imaging characteristics, etc.

[0004] Here, as a glass developed focusing on the temperature coefficient of relative refractive index, a glass composition represented by Patent Document 1 is known, for example.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2007-106611 Summary of the invention

[0008] Technical problem to be solved by the invention

[0009] The glass disclosed in Patent Document 1 contains a plurality of components forming a high refractive index, and its purpose is to increase the temperature coefficient of the relative refractive index. On the other hand, among the glasses containing a plurality of components forming a high refractive index, a glass having a small temperature coefficient of the relative refractive index has not been obtained. However, from the viewpoint of helping to correct the influence of temperature changes on imaging characteristics, a glass having a negative temperature coefficient of the relative refractive index and a glass having a small absolute value of the temperature coefficient of the relative refractive index are required.

[0010] In addition, when performing optical design, a glass material with a low refractive index and a glass material with a high refractive index and a high dispersion are sometimes joined together. When joining, the smaller the difference in the average linear thermal expansion coefficients of the glass materials combined, the better the joining. In particular, although it is known that a glass material with a low refractive index and a low dispersion containing a fluorine element has a large average linear thermal expansion coefficient, there is almost no glass material with a large average linear thermal expansion coefficient among high refractive index and high dispersion glass materials, so a glass material with a large average linear thermal expansion coefficient is required. The glass disclosed in Patent Document 1 has a small average linear thermal expansion coefficient, so it is difficult to say that it fully meets such a requirement.

[0011] In addition, the optical glass of the present invention can obtain glass having excellent visible light transmittance without the step of reheating and heat treatment to remove the coloring of the glass, and can therefore be manufactured at a lower cost.

[0012] The present invention is completed in view of the above-mentioned problems, and its purpose is to obtain an optical glass and a preform and an optical element using the optical glass, wherein the temperature coefficient of the relative refractive index of the optical glass is small, which helps to correct the influence of temperature changes on imaging characteristics, and the optical glass has an average linear thermal expansion coefficient suitable for bonding with a low-refractive-index and low-dispersion glass material.

[0013] Solutions to technical problems

[0014] The inventors of the present invention have accumulated experimental research results to solve the above technical problems and found that by containing P2O5 and Nb2O5 components and containing a predetermined amount of Na2O and K2O components, a low-priced glass with a small temperature coefficient of relative refractive index can be obtained, thereby completing the present invention. Specifically, the present invention provides the following products.

[0015] (1) An optical glass comprising, by mass %,

[0016] P2O5 content is 20.0% to 40.0%,

[0017] Nb2O5 composition is 25.0% to 50.0%,

[0018] The mass sum of (Na2O+K2O) is 3.0% to 30.0%,

[0019] The temperature coefficient (40°C to 60°C) of the relative refractive index (589.29nm) is +3.0×10 -6 (℃ -1 ) to -10.0×10 -6 (℃ -1 )’s scope.

[0020] (2) The optical glass according to (1), wherein the mass sum (Na2O+K2O+BaO) is 10.0% to 35.0%.

[0021] (3) The optical glass according to (1) or (2), wherein the average linear thermal expansion coefficient α between 100°C and 300°C is 80 (10 -7 ℃ -1 )above.

[0022] (4) The optical glass according to any one of (1) to (3), which has a refractive index (n d ), and an Abbe number (ν d ).

[0023] (5) A preform formed of the optical glass described in any one of (1) to (4).

[0024] (6) An optical element comprising the optical glass according to any one of (1) to (4).

[0025] (7) An optical device comprising the optical element described in (6).

[0026] Effects of the Invention

[0027] According to the present invention, an optical glass having a small temperature coefficient of relative refractive index, which helps to correct the influence of temperature changes on imaging characteristics and has good visible light transmittance, as well as a preform and an optical element using the optical glass can be obtained at a lower price. DETAILED DESCRIPTION

[0028] The optical glass of the present invention contains, by mass%, a P2O5 component of 20.0% to 40.0%, a Nb2O5 component of 25.0% to 50.0%, a Na2O component and a K2O component of 3.0% to 30.0%, and a relative refractive index (589.29 nm) having a temperature coefficient (40°C to 60°C) of +3.0×10 -6 (℃ -1 ) to -10.0×10 -6 (℃ -1 ) within the range of .

[0029] By containing a large amount of Na2O component and K2O component, it is possible to obtain a glass material having a small value of the temperature coefficient of relative refractive index and a large average linear thermal expansion coefficient.

[0030] Therefore, an optical glass with good visible light transmittance, a small value of the temperature coefficient of relative refractive index, which helps to correct the influence of temperature changes on imaging characteristics, has good bonding properties with low refractive index and low dispersion glass materials, and has good visible light transmittance, as well as a preform and an optical element using the optical glass can be obtained at a lower price.

[0031] Hereinafter, the embodiments of the optical glass of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and can be appropriately changed and implemented within the scope of the purpose of the present invention. In addition, although there are cases where the description of the repeated description is appropriately omitted, the main purpose of the invention is not limited thereto.

[0032] [Glass composition]

[0033] The composition ranges of the components constituting the optical glass of the present invention are as follows. In this specification, the content of each component is expressed in mass % relative to the total mass of the oxide conversion composition unless otherwise specifically denied. Here, "oxide conversion composition" means that the oxides, composite salts, metal fluorides, etc. used as raw materials for the glass components of the present invention are assumed to be completely decomposed into oxides when melted. In this case, the total mass of the generated oxides is recorded as 100 mass % to express the composition of the various components contained in the glass.

[0034] <About essential ingredients and optional ingredients>

[0035] P2O5 is an essential component as a glass-forming oxide. In particular, by containing 20.0% or more of P2O5, the viscosity of the molten glass can be improved and the stability of the glass can be improved. Furthermore, the devitrification during reheating and pressing is good. Therefore, the content of P2O5 is preferably 20.0% or more, more preferably greater than 21.0%, and even more preferably greater than 22.0%.

[0036] On the other hand, by making the content of P2O5 component 40.0% or less, the desired refractive index and dispersion can be maintained. Therefore, the content of P2O5 component is preferably 40.0% or less, more preferably 35.0% or less, and even more preferably less than 30.0%.

[0037] The P2O5 component can use Al(PO3)3, Ca(PO3)2, Ba(PO3)2, BPO4, H3PO4, NaH2PO4, KH2PO4, etc. as raw materials.

[0038] The Nb2O5 component is a high refractive index and high dispersion component and is an essential component. In particular, by containing 25.0% or more of the Nb2O5 component, the stability of the glass can be improved while maintaining a high refractive index and high dispersion. Therefore, the content of the Nb2O5 component is preferably 25.0% or more, more preferably greater than 28.0%, and even more preferably greater than 30.0%.

[0039] On the other hand, by making the content of Nb2O5 component 50.0% or less, the average linear thermal expansion coefficient is large, and the required refractive index and dispersion can be maintained. Therefore, the content of Nb2O5 component is preferably 50.0% or less, and more preferably 47.0% or less.

[0040] The Nb2O5 component can use Nb2O5 or the like as a raw material.

[0041] The Na2O component is an optional component. When the content thereof is greater than 0%, the meltability of the glass raw material can be improved, the transmittance can be improved, and the temperature coefficient of the relative refractive index can be reduced. Therefore, the content of the Na2O component is preferably greater than 0%, more preferably greater than 0.1%, even more preferably greater than 0.5%, further preferably greater than 1.0%, even more preferably greater than 1.5%, and even more preferably greater than 2.0%.

[0042] In particular, when the content exceeds 10.0%, the effect of reducing the temperature coefficient of relative refractive index increases and the glass solubility is also improved. Therefore, the content may be greater than 10.0%.

[0043] On the other hand, by making the content of Na2O component 35.0% or less, it is possible to reduce the reduction of glass refractive index and chemical durability (water resistance) caused by excessive content, reduce devitrification, and suppress devitrification during reheat pressing. Therefore, the content of Na2O component is preferably 35.0% or less, more preferably less than 30.0%, even more preferably less than 25.0%, and further preferably less than 20.0%.

[0044] Na2O component can use Na2CO3, NaNO3, NaF, Na2SiF6 and the like as raw materials.

[0045] The K2O component is an optional component. When the content thereof is greater than 0%, the average linear thermal expansion coefficient becomes large, the transmittance is good, and the temperature coefficient of the relative refractive index can be reduced. Therefore, the content of the K2O component is preferably greater than 0%, more preferably greater than 0.5%, still more preferably greater than 1.0%, and further preferably greater than 2.0%.

[0046] In particular, when the content is greater than 5.0%, the effect of reducing the temperature coefficient of relative refractive index is significantly increased and the stability of the glass is also improved, so it may be greater than 5.0%.

[0047] On the other hand, by making the content of K2O component 30.0% or less, the stability of the glass can be maintained and the decrease in the refractive index can be suppressed. Therefore, the content of K2O component is preferably 30.0% or less, more preferably less than 25.0%, still more preferably less than 20.0%, and further preferably less than 15.0%.

[0048] The K2O component can use K2CO3, KNO3, KF, KHF2, K2SiF6 and the like as raw materials.

[0049] BaO is an optional component. When its content is greater than 0%, it can improve the meltability of glass raw materials, reduce glass devitrification, increase the refractive index, and reduce the temperature coefficient of relative refractive index. Moreover, it is a component with low material cost and easy to melt among the components that obtain high refractive index. Therefore, the content of BaO is preferably greater than 0%, more preferably greater than 0.1%, even more preferably greater than 1.0%, and further preferably greater than 2.0%.

[0050] On the other hand, by making the content of BaO component less than 20.0%, the average linear thermal expansion coefficient becomes large, and the refractive index reduction or devitrification of the glass caused by excessive content can be reduced. Therefore, the content of BaO component is preferably less than 20.0%, more preferably less than 19.0%, and even more preferably less than 18.0%.

[0051] BaO component can use BaCO3, Ba(NO3)2, Ba(PO3)2, BaF2 and the like as raw materials.

[0052] The TiO2 component is a component that can increase the refractive index of the glass, reduce the Abbe number, and easily obtain stable glass when its content is greater than 0%. Therefore, the content of the TiO2 component is preferably greater than 0%, more preferably greater than 1.0%, even more preferably greater than 3.0%, and further preferably greater than 5.0%.

[0053] On the other hand, by making the content of TiO2 component less than 30.0%, the average linear thermal expansion coefficient can be increased, the temperature coefficient of relative refractive index can be reduced, the devitrification caused by excessive content of TiO2 component can be reduced, and the transmittance of glass to visible light (especially wavelength below 500nm) can be suppressed. Therefore, the content of TiO2 component is preferably less than 30.0%, more preferably less than 26.0%, more preferably less than 23.0%, and further preferably less than 20.0%.

[0054] As the TiO2 component, TiO2 or the like can be used as a raw material.

[0055] The SiO2 component is a glass-forming oxide component that can improve the viscosity of the molten glass when its content is greater than 0%. Therefore, the content of the SiO2 component is preferably greater than 0%, more preferably greater than 0.1%, and even more preferably greater than 0.3%.

[0056] On the other hand, by making the content of SiO2 component 5.0% or less, the glass transition point can be suppressed from rising and the refractive index can be suppressed from decreasing. Therefore, the content of SiO2 component is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably less than 1.0%.

[0057] For the SiO2 component, SiO2, K2SiF6, Na2SiF6 and the like can be used as raw materials.

[0058] The B2O3 component is an optional component used as a glass-forming oxide. When the content thereof is greater than 0%, the glass solubility can be improved.

[0059] On the other hand, by making the content of B2O3 component 5.0% or less, the temperature coefficient of relative refractive index can be reduced, and the deterioration of chemical durability can be suppressed, and the devitrification during reheating and pressing can be suppressed. Therefore, the content of B2O3 component is preferably 5.0% or less, more preferably 3.0% or less, more preferably less than 1.5%, and further preferably less than 1.3%.

[0060] The WO3 component is an optional component. When the content thereof is greater than 0%, it can reduce the coloring of the glass caused by other components forming a high refractive index, and can increase the refractive index, reduce the Abbe number, lower the glass transition point, and reduce devitrification.

[0061] On the other hand, by making the content of WO3 component less than 10.0%, the temperature coefficient of relative refractive index can be reduced, and devitrification during reheating and pressing can be reduced. Furthermore, the coloring of the glass caused by the WO3 component can be reduced, thereby improving the visible light transmittance. Therefore, the content of WO3 component is preferably less than 10.0%, more preferably less than 9.0%, more preferably less than 8.0%, further preferably less than 6.5%, and further preferably less than 5.0%.

[0062] As the WO3 component, WO3 or the like can be used as a raw material.

[0063] The ZnO component is an optional component, and when its content is greater than 0%, it can improve the solubility of the raw material, promote the degassing of the molten glass, and further improve the stability of the glass. Furthermore, it can lower the glass transition point and improve the chemical durability.

[0064] On the other hand, by making the content of the ZnO component less than 5.0%, the temperature coefficient of the relative refractive index can be reduced, and the expansion caused by heat can be reduced, the reduction of the refractive index can be suppressed, and the devitrification caused by too low viscosity can be reduced. Therefore, the content of the ZnO component is preferably less than 5.0%, more preferably less than 4.0%, more preferably less than 2.0%, further preferably less than 1.0%, and further preferably less than 0.5%. Furthermore, the ZnO component may not be contained.

[0065] As the ZnO component, ZnO, ZnF2 and the like can be used as raw materials.

[0066] ZrO2 is an optional component, and when its content is greater than 0%, it can increase the glass refractive index and reduce devitrification. Therefore, the content of ZrO2 is preferably greater than 0%, more preferably greater than 0.5%, and even more preferably greater than 1.0%.

[0067] On the other hand, by making the content of ZrO2 component less than 5.0%, the temperature coefficient of relative refractive index can be reduced, and devitrification caused by excessive ZrO2 component can be reduced. Therefore, the content of ZrO2 component is preferably less than 5.0%, more preferably less than 3.0%, more preferably less than 1.0%, and further preferably less than 0.5%. Furthermore, ZrO2 component may not be contained.

[0068] The ZrO2 component can use ZrO2, ZrF4, etc. as raw materials.

[0069] The MgO component, the CaO component, and the SrO component are optional components, and when the content thereof is greater than 0%, the refractive index, the melting property, and the devitrification resistance of the glass can be adjusted.

[0070] On the other hand, by making the contents of MgO, CaO and SrO 5.0% or less, it is possible to suppress the decrease in refractive index and reduce devitrification caused by excessive inclusion of these components. Therefore, the contents of MgO, CaO and SrO are preferably 5.0% or less, more preferably 3.5% or less, and even more preferably less than 2.0%.

[0071] The Li2O component is an optional component, and can improve the glass meltability and lower the glass transition point.

[0072] On the other hand, by reducing the content of Li2O, the refractive index of the glass is less likely to decrease, and the devitrification of the glass and the devitrification during reheating and pressing can be reduced. Therefore, the content of Li2O is preferably 5.0% or less, more preferably less than 3.0%, even more preferably less than 1.0%, and further preferably less than 0.5%.

[0073] As the Li2O component, Li2CO3, LiNO3, LiF, etc. can be used as raw materials.

[0074] The Al2O3 component and the Ga2O3 component are optional components, and when the content thereof is greater than 0%, the devitrification resistance of the molten glass can be improved.

[0075] On the other hand, by making the content of Al2O3 component or Ga2O3 component less than 10.0%, the liquidus temperature of glass can be lowered and the devitrification resistance can be improved. Therefore, the content of Al2O3 component and Ga2O3 component is preferably less than 10.0%, more preferably less than 5.0%, more preferably less than 3.0%, and further preferably less than 1.0%.

[0076] The Al2O3 component can use Al2O3, Al(OH)3, AlF3 or the like as a raw material, and the Ga2O3 component can use Ga2O3 or the like as a raw material.

[0077] The Sb2O3 component is an optional component, and when its content is greater than 0%, it can degas the molten glass.

[0078] On the other hand, by making the content of Sb2O3 component less than 1.0%, it is possible to suppress the decrease of transmittance in the short-wave region of the visible light region, overexposure of glass, and deterioration of internal quality. Therefore, the content of Sb2O3 component is preferably less than 1.0%, more preferably less than 0.5%, still more preferably less than 0.2%, and further preferably less than 0.1%.

[0079] As the Sb2O3 component, Sb2O3, Sb2O5, Na2H2Sb2O7·5H2O or the like can be used as a raw material.

[0080] The total content of Na2O and K2O is preferably 3.0% or more. Thus, it is easy to obtain glass having a small temperature coefficient of relative refractive index, a large average linear thermal expansion coefficient, and good transmittance. Therefore, the mass sum (Na2O+K2O) is preferably 3.0% or more, more preferably greater than 4.0%, even more preferably greater than 5.0%, and even more preferably greater than 6.0%.

[0081] On the other hand, by making the total content less than 30.0%, it is possible to suppress the deterioration of chemical durability and the reduction of the glass refractive index due to excessive content. Therefore, the mass sum (Na2O+K2O) is preferably less than 30.0%, more preferably less than 25.0%, and even more preferably less than 23.0%.

[0082] The total content of the Na2O component, the K2O component, and the BaO component is preferably 10.0% or more. This makes it possible to easily obtain glass having a small temperature coefficient of relative refractive index.

[0083] Therefore, the mass sum (Na2O+K2O+BaO) is preferably 10.0% or more, more preferably greater than 12.0%, still more preferably greater than 14.0%, further preferably greater than 16.0%, and further preferably greater than 17.5%.

[0084] On the other hand, by making the total content less than 35.0%, it is possible to suppress the deterioration of chemical durability, the decrease in glass refractive index due to excessive content, and the deterioration of devitrification during reheating and pressing. Therefore, the mass sum (Na2O+K2O+BaO) is preferably 35.0%, more preferably 33.0% or less, and even more preferably less than 30.0%.

[0085] The total content of the Nb2O5 component and the TiO2 component is preferably 30.0% or more. This can maintain a high refractive index and reduce the temperature coefficient of the relative refractive index.

[0086] Therefore, the mass sum (Nb2O5+TiO2) is preferably 30.0% or more, more preferably 35.0% or more, and still more preferably 40.0% or more.

[0087] On the other hand, by making the mass sum (Nb2O5+TiO2) 65.0% or less, the liquidus temperature can be lowered to obtain stable glass. Therefore, the mass sum (Nb2O5+TiO2) is preferably 65.0% or less, more preferably 63.0% or less, and even more preferably 60.0% or less.

[0088] The ratio of the total content of Na2O, K2O and BaO to the total content of B2O3 and TiO2 is preferably greater than 0.5. Thus, the temperature coefficient of relative refractive index can be reduced and the average linear thermal expansion coefficient can be increased. Therefore, the mass ratio (Na2O+K2O+BaO) / (B2O3+TiO2) is preferably greater than 0.5, more preferably greater than 0.7, and even more preferably greater than 1.0.

[0089] On the other hand, by making the mass ratio (Na2O+K2O+BaO) / (B2O3+TiO2) less than 5.5, it is possible to maintain the desired refractive index and transmittance, and obtain glass with good reheat pressing. Therefore, the mass ratio (Na2O+K2O+BaO) / (B2O3+TiO2) is preferably less than 5.5, more preferably less than 5.0, and even more preferably less than 4.8.

[0090] By making the sum (mass sum) of the contents of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba) greater than 0%, the refractive index, meltability, and resistance to devitrification of the glass can be improved. Therefore, the lower limit of the sum (mass sum) of the contents of RO components is preferably greater than 0%, more preferably greater than 0.5%, and even more preferably greater than 1.0%. On the other hand, by making the RO component less than 30.0%, the average linear thermal expansion coefficient can be increased, and the reduction in the refractive index of the glass or devitrification caused by excessive content can be reduced. Therefore, the upper limit of the sum (mass sum) of the contents of RO components is preferably less than 30.0%, more preferably less than 25.0%, and even more preferably less than 20.0%.

[0091] The La2O3 component, the Gd2O3 component, the Y2O3 component, the Yb2O3 component and the Ta2O5 component are optional components. When the content thereof is greater than 0%, the refractive index of the glass can be increased and the devitrification resistance can be improved.

[0092] On the other hand, by making the content of La2O3, Gd2O3, Y2O3, Yb2O3 and Ta2O5 less than 5.0%, the raw material cost of the optical glass can be reduced, and the melting temperature of the raw materials is reduced, so the energy required to melt the raw materials is reduced, so the manufacturing components of the optical glass can be reduced. Therefore, the content of each component is preferably less than 5.0%, more preferably less than 3.0%, more preferably less than 2.0%, and more preferably less than 1.0%.

[0093] The GeO2 component is an optional component. When the content thereof is greater than 0%, it can increase the refractive index of the glass and improve the resistance to devitrification.

[0094] However, GeO2 raw materials are expensive, and excessive GeO2 content will lead to increased production costs. Therefore, the content of GeO2 is preferably less than 10.0%, more preferably less than 5.0%, even more preferably less than 3.0%, and further preferably less than 1.0%.

[0095] As the GeO2 component, GeO2 or the like can be used as a raw material.

[0096] The Bi2O3 component is an optional component. When the content thereof is greater than 0%, it can increase the refractive index, decrease the Abbe number, and lower the glass transition point.

[0097] On the other hand, by making the content of Bi2O3 component less than 5.0%, the liquidus temperature of glass can be lowered and the devitrification resistance can be improved. Therefore, the content of Bi2O3 component is preferably less than 5.0%, more preferably less than 3.0%, and more preferably less than 1.0%. In particular, from the perspective of obtaining glass with good transmittance, it is preferably not contained.

[0098] As the Bi2O3 component, Bi2O3 or the like can be used as a raw material.

[0099] The TeO2 component is an optional component. When the content thereof is greater than 0%, the refractive index can be increased and the glass transition point can be lowered.

[0100] On the other hand, when a crucible made of platinum or a melting tank formed of platinum in contact with the molten glass is used to melt glass raw materials, there is a problem that TeO2 and platinum will alloy. Therefore, the content of TeO2 is preferably 10.0% or less, more preferably less than 5.0%, even more preferably less than 3.0%, and further preferably less than 1.0%.

[0101] As the TeO2 component, TeO2 or the like can be used as a raw material.

[0102] The SnO2 component is an optional component. When the content thereof is greater than 0%, it can reduce oxidation of the molten glass and make it clear, and can also improve the visible light transmittance of the glass.

[0103] On the other hand, by making the content of SnO2 component less than 3.0%, it is possible to reduce the glass coloring or glass devitrification caused by the reduction of molten glass. Furthermore, the alloying of SnO2 component with melting equipment (especially precious metals such as Pt) is reduced, and the service life of melting equipment can be extended. Therefore, the content of SnO2 component is preferably less than 3.0%, more preferably less than 1.0%, more preferably less than 0.5%, and more preferably less than 0.1%.

[0104] The SnO2 component can use SnO, SnO2, SnF2, SnF4 and the like as raw materials.

[0105] Furthermore, the components that make the glass clear and defoaming are not limited to the above-mentioned Sb2O3 components or SnO2 components, and clarifiers, defoaming agents or combinations thereof known in the field of glass manufacturing can be used.

[0106] The component F is an optional component. When the content thereof is greater than 0%, the Abbe number of the glass can be increased, the glass transition point can be lowered, and the devitrification resistance can be improved.

[0107] However, if the content of the F component, i.e., the total amount of F in the fluoride obtained by replacing a part or all of the oxides of one or more of the above-mentioned metal elements, exceeds 10.0%, the amount of volatilization of the F component increases, making it difficult to obtain stable optical constants and homogeneous glass. In addition, the Abbe number increases beyond necessity.

[0108] Therefore, the content of the component F is preferably 10.0% or less, more preferably less than 5.0%, still more preferably less than 3.0%, and further preferably less than 1.0%.

[0109] The F component can be contained in glass using, for example, ZrF 4 , AlF 3 , NaF, CaF 2 or the like as a raw material.

[0110] The ratio of the total content of SiO2, Al2O3 and ZnO to the total content of B2O3 and Rn2O (where Rn is one or more selected from the group consisting of Li, Na and K) is preferably 15.0 or less. By reducing this ratio, the deterioration of meltability can be suppressed.

[0111] Therefore, the mass ratio (SiO2+Al2O3+ZnO) / (B2O3+Rn2O) is preferably less than 15.0, more preferably less than 12.0, even more preferably less than 10.0, further preferably less than 8.0, further preferably less than 6.0, and even more preferably less than 5.0.

[0112] On the other hand, the mass ratio (SiO2+Al2O3+ZnO) / (B2O3+Rn2O) may be greater than 0. Thus, the temperature coefficient of the relative refractive index can be reduced and the average linear thermal expansion coefficient can be increased. Therefore, the mass ratio (SiO2+Al2O3+ZnO) / (B2O3+Rn2O) is preferably greater than 0, more preferably greater than 1.0, and even more preferably greater than 2.0.

[0113] By making the sum (mass sum) of the contents of the Rn2O components (Rn is one or more selected from the group consisting of Li, Na, and K) greater than 1.0%, the temperature coefficient of the relative refractive index can be reduced and the average linear thermal expansion coefficient can be increased. Therefore, the sum (mass sum) of the contents of the Rn2O components is preferably greater than 1.0%, more preferably greater than 1.5%, and even more preferably greater than 2.0%.

[0114] On the other hand, by making the mass sum below 30.0%, it is possible to reduce the devitrification caused by the reduction of glass viscosity while maintaining the required refractive index and dispersion. Therefore, the sum (mass sum) of the contents of the Rn2O components is preferably below 30.0%, more preferably less than 25.0%, and even more preferably less than 23.0%.

[0115] The optical glass of the present invention preferably contains two or more of the above Rn2O components. As a result, the temperature coefficient of the relative refractive index can be reduced, the transmittance is good, and the heat treatment step of reheating is unnecessary. In particular, it is preferred to contain two or more components including Na2O and K2O as Rn2O components, based on the fact that the average linear thermal expansion coefficient can be increased, the transmittance is good, and the temperature coefficient of the relative refractive index can be reduced.

[0116] The sum (mass sum) of the contents of Ln2O3 components (wherein Ln is one or more selected from the group consisting of La, Gd, Y, Yb, and Lu) is preferably 5.0% or less.

[0117] Thus, a glass having excellent devitrification resistance and good transmittance can be obtained. Therefore, the sum (mass sum) of the contents of the Ln2O3 components is preferably 5.0% or less, more preferably 3.5% or less, and even more preferably less than 2.0%.

[0118] <About ingredients that should not be contained>

[0119] Next, components that should not be contained in the optical glass of the present invention and components that are not suitable for being contained are described.

[0120] Other components may be added as needed within the range that does not impair the glass properties of the present invention. However, in addition to Ti, Zr, Nb, W, La, Gd, Y, Yb, and Lu, various transition metal components such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo have the property of coloring the glass even in a small amount when contained alone or in a composite form, and absorbing light of a specific wavelength in the visible light region. Therefore, in optical glasses using wavelengths in the visible light region, it is preferably substantially not contained.

[0121] Furthermore, since lead compounds such as PbO and arsenic compounds such as As 2 O 3 are components that impose a high burden on the environment, it is preferred that they are substantially not contained, that is, they are not contained at all except for unavoidable contamination.

[0122] In addition, Th, Cd, Tl, Os, Be and Se are considered as harmful chemical substances in recent years, and there is a tendency to avoid their use. Environmental measures must be taken not only in the glass manufacturing process, but also in the processing process and until the waste treatment after the product is manufactured. Therefore, when the environmental impact is important, it is preferred that these components are substantially not contained.

[0123] [Manufacturing method]

[0124] The optical glass of the present invention can be produced, for example, in the following manner. That is, the raw materials of the above-mentioned components are selected from high-purity raw materials used in general optical glass, such as corresponding oxides, hydroxides, carbonates, nitrates, fluorides, hydroxides, and metaphosphate compounds, and then these raw materials are uniformly mixed so that each component is within a specified content range, and the prepared mixture is placed in a platinum crucible, and according to the melting difficulty of the glass raw materials, an electric furnace is used to melt at a temperature range of 1000° C. to 1500° C. for 1 to 10 hours, and after stirring to homogenize, the temperature is lowered to an appropriate temperature, and then cast in a casting mold and slowly cooled, thereby producing the optical glass of the present invention.

[0125] <Physical properties>

[0126] The optical glass of the present invention preferably has a high refractive index and a low Abbe number (high dispersion).

[0127] In particular, the refractive index (n d ) is preferably 1.65 or more, more preferably 1.67 or more, and still more preferably 1.69 or more. d ) is preferably 2.00 or less, more preferably 1.98 or less, still more preferably 1.96 or less, and further preferably 1.95 or less.

[0128] In addition, the Abbe number (ν d ) is preferably 10.0 or more, more preferably 13.0 or more, still more preferably 15.0 or more, and further preferably 17.0 or more. d ) is preferably 35.0 or less, more preferably 34.0 or less, still more preferably 32.0 or less, and further preferably 30.0 or less.

[0129] By having such a high refractive index, a larger amount of light refraction can be obtained while realizing a thinner optical element. In addition, by having such a high dispersion, when used as a single lens, the focus can be appropriately moved according to the wavelength of light. Therefore, when an optical system is formed by combining with an optical element having low dispersion (high Abbe number), the aberration of the entire optical system can be reduced, and high imaging characteristics can be achieved.

[0130] Thus, the optical glass of the present invention can play an effective role in optical design. In particular, when constituting an optical system, in addition to achieving high imaging characteristics, it can also achieve miniaturization of the optical system and increase the degree of freedom in optical design.

[0131] The optical glass of the present invention has a low value of the temperature coefficient of relative refractive index (dn / dT).

[0132] More specifically, the upper limit of the temperature coefficient of the relative refractive index of the optical glass of the present invention is preferably +3.0×10 -6 ℃ -1 , more preferably +1.5×10 -6 ℃ -1 , and more preferably +1.0×10 -6 ℃ -1 , and can be the upper limit value or a value lower (decreasing side) than the upper limit value.

[0133] On the other hand, the lower limit of the temperature coefficient of the relative refractive index of the optical glass of the present invention is preferably -10.0×10 -6 ℃ -1 , more preferably -8.0×10 -6 ℃ -1 , and more preferably -7.0×10 -6 ℃ -1 , and can be the lower limit value or a value higher (increasing side) than the lower limit value.

[0134] Among them, as having a refractive index (n) of 1.65 or more d ), and has an Abbe number (ν d ) glass, glass with a low temperature coefficient of relative refractive index is rare, which makes it easier to correct the defocusing of the image caused by temperature changes. Therefore, by making the temperature coefficient of the relative refractive index within such a range, it can help correct the defocusing of the image caused by temperature changes.

[0135] The temperature coefficient of the relative refractive index of the optical glass of the present invention refers to the temperature coefficient of the refractive index (589.29nm) of the optical glass in air at the same temperature, which is calculated by calculating the change (℃) per 1℃ when the temperature changes from 40℃ to 60℃. -1 ) to indicate.

[0136] The average linear thermal expansion coefficient α of the optical glass of the present invention at 100°C to 300°C is preferably 80 (10 -7 ℃ -1 That is, the average linear thermal expansion coefficient α of the optical glass of the present invention at 100°C to 300°C is preferably 80 (10 -7 ℃ -1 ) or more, more preferably 85(10 -7 ℃ -1 ) or more, and more preferably 90 (10 -7 ℃ -1 )above.

[0137] Generally speaking, if the average linear thermal expansion coefficient α is large, the glass is prone to cracking during processing, so the average linear thermal expansion coefficient α needs to be small. On the other hand, from the perspective of combining and bonding with a glass material having a low temperature coefficient of relative refractive index and a large average linear thermal expansion coefficient α, the average linear thermal expansion coefficient α needs to be the same as or close to the value of the glass material.

[0138] Among them, in the case of having a refractive index (n d ), and has an Abbe number (ν d ) Among the glasses of the present invention, there are relatively few glass materials having a large average linear thermal expansion coefficient α. When used in combination with a glass material having a low refractive index and low dispersion, a glass having a large average linear thermal expansion coefficient α, such as that of the present invention, is more useful.

[0139] The optical glass of the present invention preferably has a high visible light transmittance, particularly a light transmittance on the medium and short wavelength sides of visible light, and has little coloration.

[0140] In particular, the optical glass of the present invention, when expressed in terms of glass transmittance, has a minimum wavelength (λ) when the spectral transmittance of a sample with a thickness of 10 mm is 80%. 80 ), preferably 460 nm or less, more preferably 450 nm or less, and still more preferably 440 nm or less.

[0141] In addition, in the optical glass of the present invention, the shortest wavelength (λ 70 ), preferably below 430 nm, more preferably below 420 nm, and still more preferably below 410 nm.

[0142] In the optical glass of the present invention, the shortest wavelength (λ5) when the spectral transmittance of a sample having a thickness of 10 mm is 5% is preferably 400 nm or less, more preferably 390 nm or less, and even more preferably 380 nm or less.

[0143] As described above, since the absorption edge of the glass is located near the ultraviolet region and the glass has high transparency to visible light, the optical glass can be preferably used as an optical element that transmits light, such as a lens.

[0144] [Preform and optical element]

[0145] A glass molded body can be produced from the produced optical glass by a grinding method, or a press molding method such as reheating and pressing molding, precision pressing molding, etc. That is, the glass molded body can be produced by the following methods: the optical glass is subjected to mechanical processing such as grinding and polishing to produce a glass molded body; or a preform for press molding is produced from the optical glass, and the preform is subjected to reheating and pressing molding, and then subjected to grinding to produce a glass molded body; or a preform produced by grinding, or a preform formed by known float molding, etc., is subjected to precision pressing to produce a glass molded body. In addition, the method of producing a glass molded body is not limited to the above methods.

[0146] Thus, the optical glass of the present invention can be used in a variety of optical elements and optical designs. It is particularly desirable to form a preform from the optical glass of the present invention, and use the preform to perform reheating press forming or precision press forming, etc., to produce optical elements such as lenses or prisms. Thus, a preform with a larger diameter can be formed, so that the optical element can be enlarged, and when used in optical equipment, high-definition and high-precision imaging characteristics and projection characteristics can be achieved.

[0147] The glass molded body formed from the optical glass of the present invention can be used for applications such as lenses, prisms, mirrors and other optical elements, and can be typically used for equipment that is prone to high temperatures, such as vehicle-mounted optical equipment, projectors, and copiers.

[0148] [Example]

[0149] The compositions of the embodiments (No. 1 to No. 51) and the comparative examples (No. A and No. B) of the present invention, and the refractive index (n d ), Abbe number (ν d ), temperature coefficient of relative refractive index (dn / dT), average linear thermal expansion coefficient (100℃ to 300℃), transmittance (λ 80 , 70 The results of λ5) are shown in Tables 1 to 8. In addition, the following examples are for illustrative purposes only, and the present invention is not limited to these examples.

[0150] The glasses of the embodiments of the present invention and the comparative examples are made of high-purity raw materials such as oxides, hydroxides, carbonates, nitrates, fluorides, metaphosphate compounds, etc., which are commonly used in optical glasses, as raw materials for each component. These raw materials are weighed and uniformly mixed in the proportions of the compositions of the embodiments shown in the table, and then put into a platinum crucible. Depending on the melting difficulty of the glass raw materials, they are melted in an electric furnace at a temperature range of 800°C to 1300°C for 1 to 10 hours, stirred to homogenize, and then cast in a mold and slowly cooled to produce glass.

[0151] The refractive index (n d ) and Abbe number (ν d ), expressed as the measured value of the d line (587.56nm) of a helium lamp. In addition, the Abbe number (ν d ), using the above refractive index for the d line and the refractive index for the F line (486.13 nm) of the hydrogen lamp (n F ), the refractive index (n C ) value, based on the Abbe number (ν d )=[(n d -1) / (n F -n C )], and thus it is calculated.

[0152] The temperature coefficient of the relative refractive index (dn / dT) of the glass of the embodiments and comparative examples is the value of the temperature coefficient of the relative refractive index in the range of 40°C to 60°C measured for light with a wavelength of 589.29 nm using the interference method described in the Japan Optical Glass Industry Association standard JOGIS18-2008 "Method for measuring the temperature coefficient of the refractive index of optical glass".

[0153] Furthermore, the average linear thermal expansion coefficient (100°C to 300°C) of the glass of the embodiments and comparative examples is obtained by measuring the relationship between temperature and the elongation of the sample according to the Japan Optical Glass Industry Association Standard JOGIS08-2003 "Method for measuring thermal expansion of optical glass", thereby obtaining a thermal expansion curve and further calculating the average linear thermal expansion coefficient.

[0154] The glass transmittance of the embodiment is measured according to the Japan Optical Glass Industry Association Standard JOGIS02-2003. In addition, in the present invention, by measuring the transmittance of the glass, the presence and degree of coloration of the glass can be obtained. Specifically, according to JIS Z8722, the spectral transmittance of the parallel polished piece with a thickness of 10 ± 0.1 mm from 200 nm to 800 nm is measured to obtain λ 80 (wavelength when transmittance is 80%), λ 70(wavelength when the transmittance is 70%) and λ5 (wavelength when the transmittance is 5%).

[0155]

Table 1

[0156]

[0157]

Table 2

[0158]

[0159]

Table 3

[0160]

[0161]

Table 4

[0162]

[0163]

Table 5

[0164]

[0165]

Table 6

[0166]

[0167]

Table 7

[0168]

[0169]

Table 8

[0170]

[0171] The optical glass of the embodiment of the present invention contains P2O5 and Nb2O5 components and contains specified amounts of Na2O and K2O components, so that low-cost glass with a small value of the temperature coefficient of relative refractive index can be obtained.

[0172] As shown in the table, the temperature coefficient of relative refractive index of any of the optical glasses in the examples is within +1.0×10 -6 (℃ -1 ) to -10.0×10 -6 (℃ -1 ) and more specifically within +3.0×10 -6 (℃ -1 ) to -10.0×10 -6 (℃ -1 ) are all within the required range.

[0173] Furthermore, any of the optical glasses of the embodiments has a refractive index (n d) are all above 1.65, which are all within the required range. Furthermore, any of the optical glasses of the embodiments of the present invention has an Abbe number (ν d ) are all within the range of 10 to 35, which is within the required range.

[0174] Furthermore, the average linear thermal expansion coefficient (100°C to 300°C) of any of the optical glasses of the embodiments is 80 (10 -7 ℃ -1 )above.

[0175] Furthermore, the optical glass of the embodiment has a transmittance (λ 80 ) is below 460nm, the transmittance (λ 70 ) is below 430nm, and the transmittance (λ5) is below 400nm.

[0176] Furthermore, the optical glass of the example was a stable glass and was not easily devitrified during the glass production. On the other hand, the glass of Comparative Example A was devitrified and thus did not undergo vitrification.

[0177] Therefore, it can be clearly seen that the optical glass of the embodiment has a refractive index (n d ) and the Abbe number (ν d ) are all within the required range, the temperature coefficient of the relative refractive index is small, and the glass can be obtained at a lower material cost. It can be seen that the optical glass of the embodiment of the present invention is helpful for miniaturization of optical systems such as vehicle-mounted optical equipment or projectors used in high-temperature environments, and is helpful for correcting defocusing of imaging characteristics caused by temperature changes.

[0178] Furthermore, the optical glass of the embodiment of the present invention is used to form a glass block, and the glass block is ground and polished to be processed into lens and prism shapes. As a result, various lens and prism shapes can be stably processed.

[0179] Although the present invention has been described in detail above for the purpose of illustration, the purpose of this embodiment is only to serve as an example, and it should be fully understood that many changes can be made to the present invention by those having ordinary knowledge in the technical field without departing from the spirit and scope of the present invention.

Claims

1. An optical glass comprising, by mass%,: P2O5 composition is 20.0% to 40.0%; Nb2O5 content is 25.0 to 50.0%; and The Na2O content is 6.69% or more and less than 30.0%, and The mass sum (Na2O+K2O) is 7.43% to 30.0%, The mass ratio (Na2O+K2O+BaO) / (B2O3+TiO2) is 1.31 or more and 4.25 or less, The refractive index (n) is 1.82 or more and 1.95 or less. d ), The temperature coefficient of the relative refractive index of the optical glass at 589.29 nm at 40°C to 60°C is +3.0×10 -6 ℃ -1 To -10.0×10 -6 ℃ -1 range.

2. The optical glass according to claim 1, wherein: The mass sum (Na2O+K2O+BaO) is 10.0% to 35.0%.

3. The optical glass according to claim 1 or 2, wherein: The average linear thermal expansion coefficient α from 100℃ to 300℃ is 80(10 -7 ℃ -1 )above.

4. The optical glass according to any one of claims 1 to 3, wherein: Abbe number (ν d ) is greater than 10 and less than 35. 5 . A preform formed from the optical glass according to claim 1 . 6 . An optical element, made of the optical glass according to claim 1 .

7. An optical device comprising the optical element according to claim 6.