Application of composite nucleating agent in preparation of microcrystalline glass, microcrystalline glass and preparation method of microcrystalline glass
By using TiO2 and ZrO2 composite nucleating agents in glass-ceramics, nano-sized ZnAl2O4 and MgAl2O4 crystals are generated, resolving the contradiction between transparency and hardness in glass-ceramics. This enables the preparation of glass-ceramics with high transparency and high hardness, expanding its application range.
Patent Information
- Application Number
- CN202411156583.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
Existing microcrystalline glass, while maintaining high transparency, has difficulty simultaneously increasing hardness. There is a contradiction between transparency and crystallinity, which limits its application range.
By using TiO2 and ZrO2 as composite nucleating agents and optimizing their content and ratio in glass-ceramics, a large number of nano-sized ZnAl2O4 and MgAl2O4 crystals are formed. Combined with the ZrO2 subcrystalline phase, the heat treatment process is optimized to generate glass-ceramics with high hardness and high transparency.
This achievement enables microcrystalline glass to achieve a high transmittance of over 80% in the visible light range, while maintaining a microhardness higher than 8.5 GPa, thus resolving the contradiction between transparency and hardness and expanding its application range.
Smart Images

Figure CN118908576A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of microcrystalline glass materials, and in particular to the application of a composite crystal nucleating agent in the preparation of microcrystalline glass, microcrystalline glass and a preparation method thereof. Background Art
[0002] Glass-ceramics are polycrystalline solid materials containing a certain amount of microcrystals, which are formed by controlling the nucleation and crystallization of precursor glass through a certain procedure of heat treatment. They have many advantages such as high mechanical strength, adjustable thermal expansion and chemical corrosion resistance, and can be used in optics, electricity and biology. For many potential applications, the transparency and strength of glass-ceramics are very important. Therefore, glass-ceramics made of spinel system glass have received more and more attention. On the one hand, spinel glass-ceramics are nanocrystalline. Even if the composition of the precursor glass changes significantly, the size of the spinel crystal is still 5-50nm, which is smaller than the wavelength of visible light, reducing the scattering of light, so that the glass-ceramics can maintain a high transparency in the visible light region. On the other hand, the spinel crystal itself has a high strength, so that the precipitation of spinel crystals in the glass matrix can potentially improve the mechanical properties of glass-ceramics. Unfortunately, due to the contradiction between crystallinity and transmittance in glass-ceramics, even if the size of the precipitated spinel crystals is small, the transparency of glass-ceramics will still be significantly reduced, which greatly limits its application range. How to further improve the surface hardness of spinel glass-ceramics while meeting high transparency is a current research hotspot. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide an application of a composite nucleus agent in the preparation of microcrystalline glass, microcrystalline glass and its preparation method. By using the composite nucleus agent of the present invention, microcrystalline glass with high transparency and high hardness can be obtained.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides an application of a composite crystal nucleus agent in the preparation of microcrystalline glass. The composite crystal nucleus agent is TiO2 and ZrO2. The content of the composite crystal nucleus agent in the microcrystalline glass is 3-9 mol%.
[0006] Preferably, the molar ratio of TiO2 to ZrO2 is 1-4:2-5.
[0007] The present invention also provides a microcrystalline glass, which is prepared by heat treatment of a precursor glass including the following contents: SiO2: 45-55mol%, Al2O3: 24-28mol%, ZnO: 6-11mol%, MgO: 4-8mol%, Li2O: 3-8mol%, Na2O: 1-5mol%, TiO2: 1-4mol%, and ZrO2: 2-5mol%.
[0008] Preferably, the main crystalline phase of the microcrystalline glass is ZnAl2O4 and MgAl2O4 crystals, and the secondary crystalline phase is ZrO2 crystals; the crystalline phase content is 40-50%.
[0009] The present invention also provides a method for preparing the microcrystalline glass described in the above technical solution, comprising the following steps:
[0010] mixing glass raw materials to obtain a mixed material;
[0011] Melting the mixture to obtain a glass melt;
[0012] The glass melt is sequentially molded and annealed to obtain a precursor glass;
[0013] The precursor glass is heat-treated to obtain glass-ceramics.
[0014] Preferably, the melting temperature is 1550-1650° C.; and the melting time is 2-4 hours.
[0015] Preferably, the annealing temperature is 500-600° C., and the holding time is 2-6 hours.
[0016] Preferably, the heat treatment comprises nucleation and crystallization performed sequentially.
[0017] Preferably, the nucleation temperature is 650-700° C., the holding time at the nucleation temperature is 3-6 hours, and the heating rate from room temperature to the nucleation temperature is 2-5° C. / min.
[0018] Preferably, the crystallization temperature is 840-960° C., the holding time at the crystallization temperature is 1-3 h, and the heating rate from the nucleation temperature to the crystallization temperature is 2-5° C. / min.
[0019] The present invention provides an application of a composite crystal nucleating agent in the preparation of microcrystalline glass. The present invention uses TiO2 and ZrO2 to form the composite crystal nucleating agent, and generates a large number of nano-scale grains whose main crystal phases are ZnAl2O4 and MgAl2O4 by optimizing the total content of the composite crystal nucleating agent. Such spinel grains have high intrinsic hardness and nano-scale grain sizes smaller than the wavelength of visible light, so that the microhardness of the prepared spinel microcrystalline glass is higher than 8.5GPa, and the average transmittance in the visible light range is about 80%. The spinel microcrystalline glass prepared by the present invention overcomes the contradiction between transmittance and crystallinity, and simultaneously achieves high hardness and high transmittance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1The DSC spectra of the precursor glasses with different contents of the composite crystal nucleating agent in Example 1 and Example 2;
[0021] Figure 2 XRD patterns of the spinel glass-ceramics prepared in Example 1 and Example 2;
[0022] Figure 3 The SEM microscopic morphology of the spinel glass-ceramics prepared in Example 1 and Example 2;
[0023] Figure 4 The transmittance curves of the spinel glass-ceramics prepared in Example 1 and Example 2 and the precursor glass in the preparation process at wavelengths of 300 to 800 nm;
[0024] Figure 5 Microhardness images of the spinel glass-ceramics prepared in Example 1 and Example 2 and the precursor glass during the preparation process. DETAILED DESCRIPTION
[0025] The present invention provides an application of a composite nucleating agent in the preparation of glass-ceramics, wherein the composite nucleating agent is TiO2 and ZrO2; the content of the composite nucleating agent in the glass-ceramics is 3-9 mol%, more preferably 3-7 mol%. In the present invention, the molar ratio of TiO2 to ZrO2 is preferably 1-4:2-5, more preferably 0.5-2:1, and further preferably 1-1.5:1. In the present invention, the glass-ceramics is preferably spinel glass-ceramics.
[0026] In the present invention, when the content of the nucleating agent is insufficient, the number of nuclei formed in the nucleation stage is insufficient, and the crystallization mechanism of the glass tends to surface crystallization, which will cause uneven distribution of grains and coarsening of grains, thereby greatly reducing the optical and mechanical properties of the microcrystalline glass; excessive use of the nucleating agent will bring about problems such as uncontrollable crystallization process, such as uncontrollable devitrification during the cooling and molding process of the glass liquid from the molten state. The present invention solves the contradiction between crystallinity and transmittance in microcrystalline glass by optimizing the content of the nucleating agent, which is of great benefit to the preparation of microcrystalline glass with high transparency and high strength.
[0027] The present invention provides a microcrystalline glass, which is prepared by heat treatment of a precursor glass including the following contents: SiO2: 45-55mol%, Al2O3: 24-28mol%, ZnO: 6-11mol%, MgO: 4-8mol%, Li2O: 3-8mol%, Na2O: 1-5mol%, TiO2: 1-4mol%, and ZrO2: 2-5mol%.
[0028] In the present invention, the composition of the precursor glass preferably includes: SiO2: 46~50mol%, Al2O3: 26~27mol%, ZnO: 7~9mol%, MgO: 4~6mol%, Li2O: 4~6mol%, Na2O: 2~4mol%, TiO2: 2~3mol%, ZrO2: 3~4mol%.
[0029] In a specific embodiment of the present invention, the main crystalline phase of the microcrystalline glass is ZnAl2O4 and MgAl2O4 crystals, and the secondary crystalline phase is ZrO2 crystals; the crystalline phase content is 40-50%.
[0030] In a specific embodiment of the present invention, the microhardness of the glass-ceramics is higher than 8.5 GPa, and the average transmittance in the visible light range is higher than 80%.
[0031] The present invention provides a method for preparing the microcrystalline glass described in the above technical solution, comprising the following steps:
[0032] The precursor glass is heat-treated to obtain the microcrystalline glass.
[0033] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0034] In the present invention, the precursor glass is preferably prepared by a method comprising the following steps:
[0035] mixing glass raw materials to obtain a mixed material;
[0036] Melting the mixture to obtain a glass melt;
[0037] The glass melt is sequentially molded and annealed to obtain the precursor glass.
[0038] The present invention mixes glass raw materials to obtain a mixture. In the present invention, the glass raw materials preferably include SiO2, Al2O3, ZnO, MgO, Li2CO3, Na2CO3, TiO2 and ZrO2. The present invention has no special restrictions on the specific composition of the glass raw materials, as long as they can form the precursor glass; the purity of the glass raw materials is preferably analytically pure, and the particle size is preferably at the micron level.
[0039] After obtaining the mixture, the present invention melts the mixture to obtain a glass melt. In the present invention, the melting temperature is preferably 1550-1650°C, more preferably 1600-1620°C; the melting time is preferably 2-4 hours, more preferably 3-3.5 hours. In the present invention, the melting is preferably carried out in a quartz crucible.
[0040] After obtaining the glass melt, the present invention sequentially shapes and anneals the glass melt to obtain a precursor glass. In the present invention, the shaping is preferably casting; the shaping preferably includes: pouring the glass melt into a preheated graphite mold for shaping. In the present invention, the preheating temperature of the graphite mold is preferably 500-650°C, more preferably 630°C.
[0041] In the present invention, the annealing temperature is preferably 500-600°C, more preferably 550-580°C; the holding time is preferably 2-6h, more preferably 2h. In the present invention, after the annealing, the glass precursor is preferably cooled to room temperature in the furnace to obtain the glass precursor.
[0042] After obtaining the precursor glass, the present invention heat treats the precursor glass to obtain glass-ceramics. In the present invention, the heat treatment preferably includes nucleation and crystallization performed in sequence. In the present invention, the atmosphere of the heat treatment is preferably an air atmosphere.
[0043] In the present invention, the nucleation temperature is preferably 650-700°C, more preferably 660-680°C; the holding time at the nucleation temperature is preferably 3-6h, more preferably 4-5h; the heating rate from room temperature to the nucleation temperature is preferably 2-5°C / min, more preferably 3-5°C / min. In the present invention, the crystallization temperature is preferably 840-960°C, more preferably 860-900°C; the holding time at the crystallization temperature is preferably 1-3h, more preferably 2-2.5h; the heating rate from the nucleation temperature to the crystallization temperature is preferably 2-5°C / min, more preferably 3-5°C / min.
[0044] In the present invention, it is preferred that the heat treatment be followed by natural cooling to room temperature to obtain glass-ceramics.
[0045] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] Example 1
[0047] The ingredients of the precursor glass are formulated according to the following molar percentages: SiO2: 46.78%, Al2O3: 26.46%, ZnO: 8.79%, MgO: 4.52%, Li2O: 4.56%, Na2O: 4.43%, TiO2: 2.23%, ZrO2: 2.23%, among which the molar ratio of the composite nucleating agent TiO2:ZrO2 is 1:1, and the total molar percentage of TiO2+ZrO2 is 4.46%.
[0048] The weight percentage is calculated according to the molar percentage of the above composition, and then the raw materials SiO2, Al2O3, ZnO, MgO, Li2CO3, Na2CO3, TiO2 and ZrO2 are weighed, the prepared powders are evenly mixed, and melted and clarified in a high-temperature furnace at 1550°C for 3 hours; the prepared glass melt is poured into a graphite mold preheated to 630°C for shaping, and then annealed in a muffle furnace at 600°C for 2 hours and cooled to room temperature with the furnace; the obtained precursor glass 1 is cut into 1 mm thick slices, heated to 680°C at a heating rate of 5°C / min and kept warm for 3 hours, and then heated to 860°C at a heating rate of 5°C / min and kept warm for 1 hour, and finally naturally cooled to room temperature to obtain a spinel microcrystalline glass with the main crystalline phase being ZnAl2O4 and MgAl2O4 nano-grains and the secondary crystalline phase being ZrO2 nanocrystals, which is recorded as microcrystalline glass 1.
[0049] Example 2
[0050] The ingredients of the precursor glass are formulated according to the following molar percentages: SiO2: 46.29%, Al2O3: 26.18%, ZnO: 8.7%, MgO: 4.46%, Li2O: 4.52%, Na2O: 4.39%, TiO2: 2.73%, ZrO2: 2.73%, among which the molar ratio of the composite nucleating agent TiO2:ZrO2 is 1:1, and the total molar percentage of TiO2+ZrO2 is 5.46%.
[0051] The weight percentage is calculated according to the molar percentage of the above precursor glass composition, and then the raw materials SiO2, Al2O3, ZnO, MgO, Li2CO3, Na2CO3, TiO2 and ZrO2 are weighed, the prepared powders are evenly mixed, and melted and clarified in a high-temperature furnace at 1600°C for 3.5 hours; the prepared glass melt is poured into a graphite mold preheated to 630°C for shaping, and then annealed in a muffle furnace at 580°C for 2 hours and cooled to room temperature with the furnace; the obtained precursor glass 2 is cut into 1 mm thick slices, heated to 700°C at a heating rate of 3°C / min and kept warm for 3 hours, and then heated to 845°C at a heating rate of 5°C / min and kept warm for 1 hour, and finally naturally cooled to room temperature to obtain a spinel microcrystalline glass with the main crystalline phase being ZnAl2O4 and MgAl2O4 nano-grains and the secondary crystalline phase being ZrO2 nanocrystals, which is recorded as microcrystalline glass 2.
[0052] Figure 1 From the DSC spectra of the precursor glasses with different contents of composite nucleating agents in Example 1 and Example 2, it can be seen that the nucleation temperature of precursor glass 1 is 690°C and the crystallization temperature is 860°C, and the nucleation temperature of precursor glass 2 is 694°C and the crystallization temperature is 845°C.
[0053] The prepared spinel glass-ceramics were polished and their performance was tested. Figure 2 The XRD spectrum of the spinel glass-ceramics shows that the crystal phase content of glass-ceramics 1 is 47.10%, and the crystal phase content of glass-ceramics 2 is 47.68%; Figure 3 This is the SEM image of the spinel glass-ceramics. It can be seen that the precipitated crystals have reached nanoscale size and are evenly distributed. Figure 4 The transmittance curves of the spinel glass-ceramics prepared in Example 1 and Example 2 and the precursor glass in the preparation process at wavelengths of 300 to 800 nm show that the average transmittance of the glass-ceramics 1 in the visible light region is 79.312%, and the average transmittance of the glass-ceramics 2 in the visible light region is 82.681%; Figure 5 The microhardness images of the spinel glass-ceramics prepared in Example 1 and Example 2 and the precursor glass in the preparation process show that the microhardness of the glass-ceramics 1 is 9.39 GPa, and the microhardness of the glass-ceramics 2 is 9.03 GPa.
[0054] Example 3
[0055] The precursor glass is formulated according to the following molar percentages: SiO2: 45.80%, Al2O3: 25.90%, ZnO: 8.61%, MgO: 4.43%, Li2O: 4.46%, Na2O: 4.34%, TiO2: 3.23%, ZrO2: 3.23%, among which the molar ratio of the composite nucleating agent TiO2:ZrO2 is 1:1, and the total molar percentage of TiO2+ZrO2 is 6.46%.
[0056] The weight percentage is calculated according to the molar percentage of the above-mentioned precursor glass composition, and then the raw materials SiO2, Al2O3, ZnO, MgO, Li2CO3, Na2CO3, TiO2 and ZrO2 are weighed, the prepared powders are evenly mixed, and melted and clarified in a high-temperature furnace at 1650°C for 4 hours; the prepared glass melt is poured into a graphite mold preheated to 630°C for shaping, and then annealed in a muffle furnace at 600°C for 2 hours and cooled to room temperature with the furnace; the obtained precursor glass is cut into 1 mm thick slices, heated to 700°C at a heating rate of 5°C / min and kept warm for 4 hours, and then heated to 840°C at a heating rate of 5°C / min and kept warm for 2 hours, and finally naturally cooled to room temperature to obtain a spinel microcrystalline glass with the main crystalline phase being ZnAl2O4 and MgAl2O4 nano-grains, and the secondary crystalline phase being ZrO2 and a small amount of TiO2 nanocrystals.
[0057] The prepared spinel glass-ceramics were polished and tested for performance. The crystal phase content of the spinel nano-glass-ceramics was 48.48%, the average transmittance in the visible light region was 78.469%, and the microhardness was 9.29 GPa.
[0058] Example 4
[0059] The precursor glass is formulated according to the following molar percentages: SiO2: 45.56%, Al2O3: 25.76%, ZnO: 8.56%, MgO: 4.39%, Li2O: 4.44%, Na2O: 4.32%, TiO2: 2.32%, ZrO2: 4.65%, among which the molar ratio of the composite nucleating agent TiO2:ZrO2 is 1:2, and the total molar percentage of TiO2+ZrO2 is 6.97%.
[0060] The weight percentage is calculated according to the molar percentage of the above-mentioned precursor glass composition, and then the raw materials SiO2, Al2O3, ZnO, MgO, Li2CO3, Na2CO3, TiO2 and ZrO2 are weighed, the prepared powders are evenly mixed, and melted and clarified in a high-temperature furnace at 1650°C for 3 hours; the prepared molten glass is poured into a graphite mold preheated to 630°C for shaping, and then annealed in a muffle furnace at 500°C for 2 hours and cooled to room temperature with the furnace; the obtained precursor glass is cut into 1 mm thick slices, heated to 650°C at a heating rate of 5°C / min and kept warm for 6 hours, and then heated to 860°C at a heating rate of 5°C / min and kept warm for 2 hours, and finally naturally cooled to room temperature to obtain spinel microcrystalline glass with the main crystalline phase being ZnAl2O4 and MgAl2O4 nano-grains and the secondary crystalline phase being ZrO2.
[0061] The prepared spinel glass-ceramics were polished and tested for performance. The crystal phase content of the spinel nano-glass-ceramics was 46.06%, the average transmittance in the visible light region was 78.0%, and the microhardness was 8.92 GPa.
[0062] Example 5
[0063] The ingredients of the precursor glass are formulated according to the following molar percentages: SiO2: 46.75%, Al2O3: 26.50%, ZnO: 8.79%, MgO: 4.51%, Li2O: 4.56%, Na2O: 4.43%, TiO2: 1.49%, ZrO2: 2.97%, among which the molar ratio of the composite nucleating agent TiO2:ZrO2 is 1:1.99 (approximately 1:2), and the total molar percentage of TiO2+ZrO2 is 4.46%.
[0064] The weight percentage is calculated according to the molar percentage of the above-mentioned precursor glass composition, and then the raw materials SiO2, Al2O3, ZnO, MgO, Li2CO3, Na2CO3, TiO2 and ZrO2 are weighed, the prepared powders are evenly mixed, and melted and clarified in a high-temperature furnace at 1650°C for 4 hours; the prepared glass melt is poured into a graphite mold preheated to 630°C for shaping, and then annealed in a muffle furnace at 600°C for 2 hours and cooled to room temperature with the furnace; the obtained precursor glass is cut into 1 mm thick slices, heated to 680°C at a heating rate of 2°C / min and kept warm for 6 hours, and then heated to 860°C at a heating rate of 2°C / min and kept warm for 3 hours, and finally naturally cooled to room temperature to obtain a spinel microcrystalline glass with the main crystalline phase being ZnAl2O4 and MgAl2O4 nano-grains and the secondary crystalline phase being ZrO2 nanocrystals.
[0065] The prepared spinel glass-ceramics were polished and tested for performance. The crystal phase content of the spinel nano-glass-ceramics was 48.50%, the average transmittance in the visible light region was 82.0%, and the microhardness was 8.87 GPa.
[0066] Example 6
[0067] The precursor glass is formulated according to the following molar percentages: SiO2: 45.52%, Al2O3: 25.84%, ZnO: 8.58%, MgO: 4.41%, Li2O: 4.56%, Na2O: 4.33%, TiO2: 2.29%, ZrO2: 4.47%, among which the molar ratio of the composite nucleating agent TiO2:ZrO2 is 1:1.95, and the total molar percentage of TiO2+ZrO2 is 6.76%.
[0068] The weight percentage is calculated according to the molar percentage of the above-mentioned precursor glass composition, and then the raw materials SiO2, Al2O3, ZnO, MgO, Li2CO3, Na2CO3, TiO2 and ZrO2 are weighed, the prepared powders are evenly mixed, and melted and clarified in a high-temperature furnace at 1650°C for 4 hours; the prepared glass melt is poured into a graphite mold preheated to 630°C for shaping, and then annealed in a muffle furnace at 600°C for 2 hours and cooled to room temperature with the furnace; the obtained precursor glass is cut into 1 mm thick slices, heated to 700°C at a heating rate of 3°C / min and kept warm for 3 hours, and then heated to 940°C at a heating rate of 3°C / min and kept warm for 1 hour, and finally naturally cooled to room temperature to obtain a spinel microcrystalline glass with the main crystalline phase being ZnAl2O4 and MgAl2O4 nano-grains, and the secondary crystalline phase being ZrO2 and a small amount of TiO2 nanocrystals.
[0069] The prepared spinel glass-ceramics were polished and tested for performance. The crystal phase content of the spinel nano-glass-ceramics was 48.47%, the average transmittance in the visible light region was 76.035%, and the microhardness was 8.78 GPa.
[0070] The spinel glass-ceramics prepared by the present invention overcomes the contradiction between transmittance and crystallinity, and simultaneously achieves high hardness and high transmittance. Moreover, the preparation method of the nano-spinel glass-ceramics provided by the present invention is simple and easy to operate, and can be easily converted into an industrial production process line, which is conducive to large-scale industrial production.
[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An application of a composite crystal nucleating agent in the preparation of microcrystalline glass, wherein the composite crystal nucleating agent is TiO2 and ZrO2; the content of the composite crystal nucleating agent in the microcrystalline glass is 3 to 9 mol%.
2. The use according to claim 1, characterized in that: The molar ratio of TiO2 to ZrO2 is 1-4:2-5.
3. A glass-ceramic, characterized in that: The invention is prepared by heat treating a precursor glass including the following contents: SiO2: 45-55mol%, Al2O3: 24-28mol%, ZnO: 6-11mol%, MgO: 4-8mol%, Li2O: 3-8mol%, Na2O: 1-5mol%, TiO2: 1-4mol%, and ZrO2: 2-5mol%.
4. The glass-ceramic according to claim 3, characterized in that: The main crystal phase of the microcrystalline glass is ZnAl2O4 and MgAl2O4 crystals, and the secondary crystal phase is ZrO2 crystals; the crystal phase content is 40-50%.
5. The method for preparing glass-ceramics according to claim 3 or 4, characterized in that: The following steps are involved: The precursor glass is heat-treated to obtain the microcrystalline glass.
6. The preparation method according to claim 5, characterized in that: The precursor glass is prepared by a method comprising the following steps: mixing glass raw materials to obtain a mixed material; Melting the mixture to obtain a glass melt; Sequentially shaping and annealing the glass melt to obtain the precursor glass; The melting temperature is 1550-1650° C.; the melting time is 2-4 hours.
7. The preparation method according to claim 6, characterized in that: The annealing temperature is 500-600° C., and the insulation time is 2-6 hours.
8. The preparation method according to claim 5, characterized in that: The heat treatment includes nucleation and crystallization performed sequentially.
9. The preparation method according to claim 8, characterized in that: The nucleation temperature is 650-700° C., the insulation time at the nucleation temperature is 3-6 hours, and the heating rate from room temperature to the nucleation temperature is 2-5° C. / min.
10. The preparation method according to claim 8, characterized in that: The crystallization temperature is 840-960° C., and the holding time at the crystallization temperature is 1-3 hours; the heating rate from the nucleation temperature to the crystallization temperature is 2-5° C. / min.
Citation Information
Patent Citations
Spinel transparent microcrystalline glass with low melting temperature, preparation method and performance enhancing method thereof
CN111018354A
Glass ceramic, electronic equipment and preparation method of glass ceramic
CN113526872A
Transparent colorless spinel microcrystalline glass and preparation and application thereof
CN118125715A