Calcium-based additive modified alkali-resistant zirconium-rich basalt fiber and preparation method thereof

By using calcium-based additives in the preparation of zirconium-rich basalt fibers, the melt viscosity and preparation temperature are reduced, the problems of difficult preparation and high energy consumption in the prior art are solved, the alkali resistance and mechanical properties of the fiber are improved, and the alkali resistance and mechanical properties of the fiber are achieved. Efficient and energy-saving production process.

CN118908580APending Publication Date: 2024-11-08INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411229233.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The melt viscosity of existing zirconium-rich basalt fibers during the preparation process is too high, resulting in an increase in the drawing temperature, increasing the production difficulty and production energy consumption, and affecting its alkali resistance.

Method used

By using the method of calcium-based additive modification, basalt ore is mixed with alkali-resistant additives and calcium-based additives, and after melting, clarification and homogenization, homogenizing and obtaining homogeneous zirconium-rich basalt glass, reducing melt viscosity and improving The wire drawing temperature window is controlled between 1380℃ and 1520℃ in the wire drawing operation temperature.

Benefits of technology

It significantly reduces the difficulty of preparing zirconium-rich basalt fibers and produces energy consumption, improves the mechanical properties and alkali resistance of the fibers, reduces the brushing operation temperature, increases the brushing temperature window, and significantly improves the strength retention rate of the fibers after alkali corrosion, and loses mass The rate is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908580A_ABST
    Figure CN118908580A_ABST
Patent Text Reader

Abstract

The invention discloses a calcium-based additive modified alkali-resistant zirconium-rich basalt fiber and a preparation method thereof, and belongs to the technical field of basalt fiber preparation. Aiming at the problem of how to reduce the viscosity and the preparation temperature of the zirconium-rich basalt fiber at present, basalt ore is used as a main raw material, an alkali-resistant additive zircon is combined, a calcium-based additive is used as a modifier, and homogenization is performed in a high-temperature furnace to obtain homogenized zirconium-rich basalt glass modified by the calcium-based additive. And then preparing the zirconium-rich basalt fiber with high tensile strength and excellent alkali resistance in an inorganic nonmetal fiber drawing furnace. According to the invention, the viscosity of the zirconium-rich basalt melt and the wiredrawing operation temperature of the zirconium-rich basalt fiber are reduced, and the wiredrawing temperature window is increased, so that the preparation difficulty and production energy consumption of the alkali-resistant zirconium-rich basalt fiber with excellent mechanical properties are reduced; the invention provides an effective method for large-scale and efficient production and utilization of the zirconium-rich basalt fiber with excellent alkali resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of basalt fiber preparation, and specifically relates to an alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive and a preparation method thereof. Background Art

[0002] High-tech fibers are of great significance to national construction and are an important foundation for supporting the development of high-tech industries. Basalt fiber has the characteristics of high strength, high modulus, high and low temperature resistance, chemical corrosion resistance, UV resistance, low moisture absorption, sound insulation, heat insulation, and good insulation performance. Its excellent comprehensive performance is unmatched by other high-performance fibers. It can be widely used in civil engineering, transportation, energy and environmental protection, automobiles and ships, aerospace, petrochemicals, and weapons and equipment. However, in actual use, basalt fibers are often exposed to extreme conditions. The most common is that when basalt fibers are used as concrete reinforcement materials, the strong alkalinity of the cement matrix will cause corrosion of basalt fibers, especially in the early stages of hardening. Due to alkaline corrosion, the mechanical properties of basalt fibers and basalt fiber reinforced concrete will decrease. Therefore, how to improve the alkali resistance of basalt fibers has become one of the key issues to be solved in the field of basalt fiber reinforced concrete.

[0003] At present, the main method to improve the alkali resistance of basalt fiber is to add alkali-resistant additive ZrO2 to the raw materials during fiber preparation. After the zirconium-rich basalt fiber is corroded by alkali, a layer of ZrO2 appears on the surface. 4+ , Fe 3+ and Mg 2+ The dense protective layer composed of insoluble compounds such as alkali-resistant compounds prevents the internal fibers from contacting with alkaline media, thereby enhancing the alkali resistance of basalt fibers. The patent (publication number: CN98114321.0) discloses a raw material formula and manufacturing method for alkali-resistant basalt fibers of a multi-ore combination, using basalt, dolomite, celestite, zircon, ilmenite and other ore powders as raw materials, and preparing alkali-resistant basalt fibers through melting and drawing processes. The patent (publication number: CN 109879598A) reports a high alkali-resistant basalt fiber made of two or more basalt ores as the main raw materials and adding the alkali-resistant additive ZrO2, which has high mechanical properties and drawing stability.

[0004] Although the existing research work has achieved many results and progress, there are still problems that need to be further studied and solved: the viscosity of basalt melt is considered to be one of the most important process parameters for the production of basalt melt products. The size and stability of the viscosity directly affect the product quality and preparation difficulty of basalt fiber production. However, the addition of ZrO2 leads to a significant increase in the viscosity of the basalt melt, which increases the drawing temperature of zirconium-rich basalt fiber, increases the difficulty of fiber preparation and production energy consumption, and is not conducive to the industrial production of zirconium-rich basalt fiber.

[0005] In view of this, it is of great significance to study how to reduce the viscosity and preparation temperature of zirconium-rich basalt fibers in order to prepare high-performance zirconium-rich basalt fibers that are efficient and energy-saving. Summary of the invention

[0006] In response to the current problem of how to reduce the viscosity and preparation temperature of zirconium-rich basalt fiber, the present invention provides a raw material formula and preparation method for alkali-resistant zirconium-rich basalt fiber that is simple to prepare and has low energy consumption. The modified fiber of the present invention has high mechanical properties and alkali resistance, the drawing operation temperature is much lower than that before modification, and the drawing temperature window is significantly increased, which greatly reduces the preparation difficulty and production energy consumption of alkali-resistant zirconium-rich basalt fiber.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive comprises the following steps: Step 1, drying and crushing the basalt ore, then mixing it with an alkali-resistant additive and a calcium-based additive, melting, clarifying, homogenizing, and quenching to obtain a modified homogeneous zirconium-rich basalt glass; Step 2: preparing and drying the homogeneous zirconium-rich basalt glass fiber to obtain zirconium-rich basalt fiber modified with calcium-based additives.

[0008] Furthermore, expressed in terms of weight percentage of oxides, the chemical composition range of the homogeneous zirconium-rich basalt glass is: SiO2: 43.0%~56.0%, Al2O3: 13.0%~18.0%, CaO: 4.0%~9.0%, Fe2O3: 6.0%~13.0%, MgO: 2.0%~6.0%, TiO2: 0.5%~3.0%, Na2O+K2O: 2.0%~6.0%.

[0009] Furthermore, the basalt ore, the alkali-resistant additive and the calcium-based additive are calculated in terms of mass percentage: the basalt ore is 80% to 95%, the alkali-resistant additive is 3% to 11%, and the calcium-based additive is 1% to 15%.

[0010] Furthermore, the calcium-based additive is any one of CaO or calcium-based ore with a calcium content of not less than 90%. The addition of calcium-based additives can reduce the viscosity of the melt, thereby reducing the temperature required for wire drawing. 2+ The silicon-oxygen structure of the melt is partially destroyed, which reduces the polymerization degree of [SiO4]. This lowers the production temperature while taking into account the mechanical properties of the fiber.

[0011] Furthermore, the alkali-resistant additive is any one of ZrSiO4 (zircon) and ZrO2.

[0012] Furthermore, in step 1, the basalt ore is dried and crushed at a drying temperature of 100° C. to 140° C. for a drying time of 5 h to 10 h, and the basalt ore is crushed to a particle size of less than 80 mesh.

[0013] Furthermore, in step 1, the homogenization temperature is 1500° C. to 1600° C., and the homogenization time is 8 h to 16 h.

[0014] Furthermore, the fiber preparation in step 2 is specifically a wire drawing operation, the wire drawing operation temperature is controlled at 1380° C. to 1520° C., and the wire drawing speed is 600 m / min to 1300 m / min.

[0015] Furthermore, in step 2, the drying temperature is 105° C. and the drying time is 2 h.

[0016] The invention discloses an alkali-resistant zirconium-rich basalt fiber modified with a calcium-based additive prepared according to the preparation method.

[0017] Compared with the prior art, the present invention has the following advantages: The calcium-based additive used in the present invention is one of the components of basalt, which can maintain the naturalness of basalt fiber to a large extent, and is low-priced and widely available. The addition of calcium-based additives significantly reduces the viscosity of zirconium-rich basalt melt and the drawing temperature of zirconium-rich basalt fiber, thereby increasing the drawing temperature window and improving the drawing stability. Zirconium in the fiber is mainly in the form of hexacoordinated [ZrO6] and [SiO4] units connected by Si-O-Zr bonds to form ZrO6-SiO4 polyhedrons that enter the network structure, while Ca 2+ It can promote the formation of [ZrO6], so the modified zirconium-rich basalt fiber has excellent mechanical properties and alkali resistance. Thus, the production process of zirconium-rich basalt fiber is optimized, the production efficiency is improved, and the preparation difficulty and production energy consumption are reduced. The present invention provides an effective method for the large-scale and efficient production and utilization of zirconium-rich basalt fiber with excellent alkali resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 1 is a viscosity diagram of zirconium-rich basalt melts prepared in the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION

[0019] In order to gain a deeper understanding of the present invention, we will provide a comprehensive and detailed description of the present invention. However, the present invention has multiple implementations and is not limited to the specific examples listed herein. The presentation of these examples is intended to deepen the comprehensive understanding of the disclosure of the present invention.

[0020] Example 1

[0021] Zircon (ZrSiO4) was selected as an alkali-resistant additive and CaO as a calcium-based additive. By weighing and measuring, the mass percentage of each component was set to 93% of basalt ore, 6% of zircon, and 1% of CaO. The above raw materials were dried (drying temperature was 120°C, time was 6h) and mixed evenly. After melting, clarifying, and homogenizing (homogenizing temperature was 1580°C, time was 10h), homogeneous zirconium-rich basalt glass was obtained by quenching. Its chemical composition was expressed in the form of oxides, among which SiO2: 52.37%, Al2O3: 14.44%, Fe2O3: 9.75%, CaO: 7.64%, MgO: 4.54%, TiO2: 1.67%, K2O: 1.37%, Na2O: 3.14%, and ZrO2: 4.09%. 40g~60g was placed in a high temperature rotational viscometer to measure the high temperature viscosity of the melt. The crucible used for the test was a corundum crucible, the maximum furnace temperature was 1600℃, the test temperature range was 1200℃~1600℃, and the test cooling rate was 3℃ / min.

[0022] The viscosity data of the zirconium-rich basalt melt in Example 1 are as follows: Figure 1 As shown in the figure, it can be seen that the high temperature viscosity of the zirconium-rich basalt melt in Example 1 is significantly reduced. Then, alkali-resistant zirconium-rich basalt fiber is prepared in an inorganic non-metallic fiber drawing furnace. The temperature is continuously changed during the drawing process to obtain the drawing operation temperature range and the drawing temperature window.

[0023] In order to obtain fibers with stable mechanical properties and compare tensile strength, the preparation viscosity of the fibers used to test tensile strength is stabilized at 15Pa·s~25Pa·s. Table 1 shows the drawing operating temperature and drawing window temperature of zirconium-rich basalt fiber. The drawing operating temperature range of the zirconium-rich basalt fiber in this embodiment is 1405℃~1460℃, and the drawing temperature window is 55℃.

[0024] In order to simulate the corrosion environment in strong alkaline concrete, the prepared modified zirconium-rich basalt fiber was immersed in 1 mol / L NaOH solution, kept warm in a water bath at 80°C for 3 hours, taken out and ultrasonically washed 3 to 5 times in an ultrasonic cleaner with distilled water, and then placed in a glass container and dried in an oven at 105°C for 2 hours. The fiber was cooled and weighed, and the mass loss rate was calculated. The higher the mass loss rate, the worse the fiber's alkali resistance. In addition, the tensile strength of the corroded zirconium-rich basalt fiber was tested, and the strength retention rate was calculated. The higher the strength retention rate, the better the fiber's alkali resistance. The mass loss rate, initial tensile strength and strength retention rate of the fiber after the alkali resistance test are shown in Table 2. The changes in the element content of the fiber after the alkali resistance test are shown in Table 3.

[0025] The mass loss rate of the alkali-resistant zirconium-rich basalt fiber in this embodiment is 2.71%, the tensile strength of the uncorroded fiber is 1615.68 MPa, the tensile strength after corrosion is 998.26 MPa, and the strength retention rate is 61.79%.

[0026] Example 2

[0027] The difference from Example 1 is that: the weight proportion of basalt ore components is 91%, CaO 3%; Homogeneous zirconium-rich basalt glass was obtained by quenching, and its chemical composition was expressed in the form of oxides, including SiO2: 51.31%, Al2O3: 14.16%, Fe2O3: 9.59%, CaO: 9.54%, MgO: 4.42%, TiO2: 1.65%, K2O: 1.34%, Na2O: 3.07%, and ZrO2: 4.10%.

[0028] The wire drawing operating temperature range is 1385℃~1455℃, and the wire drawing temperature window is 70℃.

[0029] Under the same alkaline corrosion conditions, the mass loss rate of the alkali-resistant zirconium-rich basalt fiber of Example 2 is 2.27%, the tensile strength of the uncorroded fiber is 1816.65 MPa, the tensile strength after corrosion is 1312.00 MPa, and the strength retention rate is 72.22%.

[0030] Example 3

[0031] The difference from Example 1 is that the weight proportion of basalt ore components is 89%, CaO is 5%; Homogeneous zirconium-rich basalt glass was obtained by quenching, and its chemical composition was expressed in the form of oxides, including SiO2: 50.16%, Al2O3: 13.76%, Fe2O3: 9.32%, CaO: 11.40%, MgO: 4.34%, TiO2: 1.61%, K2O: 1.29%, Na2O: 2.98%, and ZrO2: 4.13%.

[0032] The wire drawing operating temperature range is 1377℃~1442℃, and the wire drawing temperature window is 65℃.

[0033] Under the same alkaline corrosion conditions, the mass loss rate of the alkali-resistant zirconium-rich basalt fiber of Example 3 is 2.58%, the tensile strength of the uncorroded fiber is 1734.02 MPa, the tensile strength after corrosion is 1178.32 MPa, and the strength retention rate is 67.95%.

[0034] Comparative Example 1

[0035] The difference from Example 1 is that no calcium-based additive is added, and the weight proportion of the basalt ore component is 94%.

[0036] Homogeneous zirconium-rich basalt glass is obtained by quenching, and its chemical composition is expressed in the form of oxides, including SiO2: 52.94%, Al2O3: 14.60%, Fe2O3: 9.83%, CaO: 6.79%, MgO: 4.59%, TiO2: 1.71%, K2O: 1.38%, Na2O: 3.17%, and ZrO2: 4.06%.

[0037] The wire drawing operating temperature range is 1422℃~1472℃, and the wire drawing temperature window is 50℃.

[0038] Under the same alkaline corrosion conditions, the mass loss rate of the zirconium-rich basalt fiber in Comparative Example 1 was 3.00%, the tensile strength of the uncorroded fiber was 1541.98 MPa, the tensile strength after corrosion was 883.52 MPa, and the strength retention rate was 57.30%.

[0039] Table 1 Drawing temperature and drawing temperature window of zirconium-rich basalt fiber

[0040] Table 2 Tensile strength, mass loss rate and strength retention rate of zirconium-rich basalt fiber after corrosion

[0041] Table 3 Changes in the main element contents of zirconium-rich basalt fiber before and after alkali corrosion

[0042] In summary, combined with Figure 1As shown, compared with Comparative Example 1, the mass loss rate of the alkali-resistant zirconium-rich basalt fiber of Example 1 decreased by 9.67%, the tensile strength increased by 4.78%, and the strength retention rate increased from 57.30% to 61.79%. After corrosion, the Si and Al contents on the fiber surface decreased by 7.31% and 13.51%, respectively, which were lower than 8.61% and 14.77% of the comparative example. Compared with Comparative Example 1, the mass loss rate of the alkali-resistant zirconium-rich basalt fiber of Example 2 decreased by 24.33%, the tensile strength increased by 17.81%, and the strength retention rate increased sharply from 61.79% to 72.22%. After corrosion, the Si and Al contents on the fiber surface decreased by 6.05% and 9.60%, respectively, which were significantly lower than 8.61% and 14.77% of the comparative example. Compared with Comparative Example 1, the mass loss rate of the alkali-resistant zirconium-rich basalt fiber of Example 3 decreased by 14.00%, the tensile strength increased by 12.45%, and the strength retention rate increased from 61.79% to 67.95%. After corrosion, the Si and Al contents on the fiber surface decreased by 6.95% and 11.24%, respectively, which were significantly lower than 8.61% and 14.77% of the comparative example. This shows that the mechanical properties and alkali resistance of the zirconium-rich basalt fiber of the present invention are greatly improved. Compared with comparative example 1, the wire drawing operation temperature of the zirconium-rich basalt fibers of Examples 1 to 3 is significantly reduced, and the wire drawing temperature window is increased, and the tensile strength of the prepared zirconium-rich basalt fibers is significantly increased. After the alkali resistance experiment, the fiber strength and fiber strength retention rate are significantly improved, the fiber mass loss rate is significantly reduced, and the alkali resistance is greatly enhanced. This shows that the production difficulty and energy consumption of the zirconium-rich basalt fiber of the present invention are significantly reduced, which is of great significance to the industrial production process of zirconium-rich basalt fibers.

[0043] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

Claims

1. A method for preparing alkali-resistant zirconium-rich basalt fiber modified by calcium-based additives, characterized in that: The following steps are involved: Step 1, drying and crushing the basalt ore, then mixing it with an alkali-resistant additive and a calcium-based additive, melting, clarifying, homogenizing, and quenching to obtain a modified homogeneous zirconium-rich basalt glass; Step 2: preparing and drying the homogeneous zirconium-rich basalt glass fiber to obtain zirconium-rich basalt fiber modified with calcium-based additives.

2. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: Expressed in terms of weight percentage of oxides, the chemical composition range of the homogeneous zirconium-rich basalt glass is: SiO2: 43.0%~56.0%, Al2O3: 13.0%~18.0%, CaO: 4.0%~9.0%, Fe2O3: 6.0%~13.0%, MgO: 2.0%~6.0%, TiO2: 0.5%~3.0%, and Na2O+K2O: 2.0%~6.0%.

3. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: The basalt ore, alkali-resistant additive and calcium-based additive are calculated by weight percentage: basalt ore accounts for 80% to 95%, alkali-resistant additive accounts for 3% to 11%, and calcium-based additive accounts for 1% to 15%.

4. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: The calcium-based additive is any one of CaO or calcium-based ore with a calcium content of not less than 90%.

5. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: The alkali-resistant additive is any one of ZrSiO4 and ZrO2.

6. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: In the step 1, the basalt ore is dried and crushed at a drying temperature of 100° C. to 140° C. for a drying time of 5 h to 10 h, and the basalt ore is crushed to a particle size of less than 80 mesh.

7. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: In step 1, the homogenization temperature is 1500° C. to 1600° C., and the homogenization time is 8 h to 16 h.

8. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: The fiber preparation in step 2 is specifically performed by wire drawing, the wire drawing temperature is controlled at 1380° C. to 1520° C., and the wire drawing speed is 600 m / min to 1300 m / min.

9. The method for preparing the alkali-resistant zirconium-rich basalt fiber modified by a calcium-based additive according to claim 1, characterized in that: The drying temperature in step 2 is 105° C. and the drying time is 2 h.

10. An alkali-resistant zirconium-rich basalt fiber modified with a calcium-based additive obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • High-temperature-resistant basalt fiber as well as preparation method and application thereof

    CN120208538A