AG glass and etching processing method thereof
By using the appropriate film and printed screen to perform screen printing of acid-resistant protective ink layer in glass etching, the texture control and cost problems of glass etching in the prior art are solved, high flatness and AG effect are achieved, and the Hydrophobic properties of glass.
Patent Information
- Application Number
- CN202411239857.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
AI Technical Summary
The existing glass etching technology has problems such as large tolerances in texture size, difficulty in controlling transparency, expensive exposure and development, and inconvenient operation, resulting in a single appearance and poor effect of the glass.
By making film and printing screens that adapt to glass size and shape, the front camera hole position of the glass substrate is protected by using direct screen printing acid-resistant protection ink layer to avoid the influence of etching liquid, and remove the ink layer after etching to ensure the glass surface flatness and AG effect.
The high flatness and AG effect of the glass surface are achieved, the process is simplified, the cost is reduced, the product grade is improved, and the glass is given superhydrophobic characteristics, enhancing self-cleaning, anti-icing and anti-condensing properties.
Smart Images

Figure BDA0005028910200000091 
Figure BDA0005028910200000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of glass processing, and in particular to AG glass and an etching processing method thereof. Background Art
[0002] With the advent of the 5G era, glass is widely used in the shells of electronic products such as mobile phones. Considering that the homogenization of electronic products on the market is particularly serious, that is, the glass appearance structure of existing electronic products is not much different, which has caused aesthetic fatigue among users. In order to break the deadlock of single product appearance and serious homogenization, existing technicians usually modify the glass to form etched patterns on its surface, so that the glass appearance presents AG effects such as matte, glossy, and shiny sand.
[0003] There are two main types of etching patterns on the surface of glass on the market: one is formed by high-temperature hot pressing of molds. Although this method can form concave and convex textures on the glass to obtain AG effect, the resulting texture size tolerance is large, and it is difficult to control the consistency and transparency of the texture, so the resulting product is of low grade and poor effect. The other is the acid etching method to obtain AG effect. Before etching the glass, the non-etched part will be masked. The general masking method is to spray photosensitive ink on the glass surface and then expose and develop it. However, the exposure and development method is expensive and inconvenient to operate. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes an AG glass and an etching processing method thereof. By making a film and a printing screen that are suitable for the size and shape of the glass, the camera holes on the front of the glass substrate are effectively avoided and protected by directly silk-screening an acid-resistant protective ink layer, and then the glass substrate is etched to ensure that an effective AG effect is formed in the appropriate area on the front of the glass substrate.
[0005] The present invention provides an etching method for AG glass, comprising the following steps:
[0006] S1, manufacturing the first and second films according to the external dimensions of the front and back surfaces of the glass substrate, wherein the first film also has a light-transmitting hole corresponding to the camera hole position on the front surface of the glass substrate;
[0007] S2, making a printing screen according to the first and second films, and using the printing screen to screen print an acid-resistant protective ink layer on the camera hole position on the front side of the glass substrate and the entire area on the back side;
[0008] S3, immersing the glass substrate with the acid-resistant protective ink layer printed on it in the etching solution, and etching the area on the glass substrate not covered by the acid-resistant ink layer to produce an AG effect;
[0009] S4. Immerse the glass substrate etched with the AG effect in a deplating solution to remove the acid-resistant ink layer on the glass substrate.
[0010] In the present invention, by manufacturing a first film sheet corresponding to the camera hole position on the front side of the glass substrate, and manufacturing a printing screen according to the first film sheet, an acid-resistant protective ink layer accurately positioned on the camera hole position can be screen-printed on the printing screen, and then etching treatment is performed, so that the avoidance area can be accurately positioned and the corresponding position can be protected from being treated by the etching liquid during AG treatment; at the same time, the acid-resistant protective ink layer is used in coordination with the subsequent AG treatment, which can effectively avoid the phenomenon that the protective layer falls off and the surface of the avoidance area is etched due to the presence of strong acidic substances in the etching liquid during the subsequent AG treatment, thereby ensuring effective protection of the covered area, and other front areas outside the covered area can be completely and effectively AG anti-glare treated.
[0011] Preferably, the size of the light-transmitting hole on the first film is 0.05-2 mm larger than the camera hole.
[0012] Preferably, the thickness of the acid-resistant protective ink layer is 15-25 μm;
[0013] Preferably, the screen printing rate is 150-350 mm / s, the ink return rate is 200-400 mm / s, and the screen printing pressure is 0.3-0.5 MPa.
[0014] Preferably, the acid-resistant ink layer is formed by curing at 120-150° C. for 5-8 minutes.
[0015] In the present invention, the acid-resistant protective ink layer can be well cured and adhered to the surface of the corresponding camera hole position by curing treatment at 120-150°C.
[0016] Preferably, the etching solution comprises, by mass percentage, 20-25% ammonium hydrofluoride, 10-15% oxalic acid, 15-20% ammonium sulfate, 20-25% barium sulfate, 5-10% glycerol, and the balance water.
[0017] In the present invention, the etching liquid directly contains strong acidic substances such as hydrofluoric acid, which can ensure that the surface of the glass substrate is etched to achieve an anti-glare effect, and the strong acid will not corrode the ink layer during the etching process to affect its adhesion or directly cause it to fall off, effectively ensuring the protection of the area corresponding to the camera hole position on the glass substrate, and also preventing the etching liquid from penetrating and affecting its surface due to poor adhesion.
[0018] Preferably, the etching temperature is 30-40° C. and the etching time is 1-2 min.
[0019] Preferably, the deplating solution is a sodium hydroxide or potassium hydroxide solution;
[0020] Preferably, the concentration of the sodium hydroxide or potassium hydroxide solution is 5-10 wt %.
[0021] Preferably, after step S4, the method further includes: spraying a hydrophobic coating on the front side of the glass substrate to form a hydrophobic layer on the front side of the glass substrate.
[0022] Preferably, the hydrophobic coating comprises, by mass percentage, 15-20% of fluorinated modified organic silica sol, 10-15% of polytetrafluoroethylene powder, 0.5-1% of leveling agent, and the balance is ethanol.
[0023] In the present invention, there is an uneven microstructure on the front side of the glass substrate after etching. At this time, the fluorinated modified organic silicon sol in the hydrophobic coating can be effectively deposited on the front side of the glass substrate after spraying, and there are similar compatible groups between the fluorinated modified organic silicon sol and the nano-scale polytetrafluoroethylene powder, which can improve the effective deposition and bonding of the hydrophobic layer of the polytetrafluoroethylene structure on the surface of the glass substrate, giving the glass surface excellent hydrophobicity and self-cleaning properties.
[0024] The present invention also provides an AG glass, which is prepared by the above processing method.
[0025] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0026] On the one hand, the acid-resistant protective ink layer is directly screen-printed by making a film and a printing screen to replace the exposure and development of photosensitive ink to protect the glass substrate. The process is simple and the shielding performance is good.
[0027] On the other hand, an acid-resistant ink layer is first used to protect the avoidance area corresponding to the camera hole position, and then an AG anti-glare etching treatment is performed. This can effectively prevent the corresponding camera hole position area on the glass substrate from forming a rough granular surface, and retain the original smoothness and flatness of the glass substrate surface.
[0028] On the other hand, by spraying hydrophobic coating, the surface of the glass substrate is modified with low surface energy materials, so that the glass can obtain better super-hydrophobic properties. In this way, the glass surface can have better self-cleaning, anti-icing, anti-frost, anti-condensation and other effects, further ensuring the comprehensive performance of the glass surface and making the glass more applicable. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described in detail below through specific embodiments. However, it should be clear that these embodiments are provided for illustration and are not to be construed as limiting the scope of the present invention.
[0030] Example 1
[0031] This embodiment provides an etching method for AG glass, and the preparation method includes the following steps:
[0032] (1) providing a transparent glass substrate, ultrasonically cleaning the glass substrate with acetone and ethanol for 5 minutes in sequence, then rinsing it with deionized water, and drying it for later use;
[0033] (2) manufacturing a first film and a second film according to the outer dimensions of the front and back surfaces of the glass substrate, wherein the first film has a light-transmitting hole corresponding to the camera hole position on the front surface of the glass substrate and having a size 1 mm larger;
[0034] (3) The first film and the second film are exposed to light through a silk screen to produce a first printing screen and a second printing screen respectively, wherein only hollows corresponding to the light-transmitting holes are left on the first screen;
[0035] (3) using a first printing screen and a second printing screen to respectively screen-print the acid-resistant protective ink R568 on the front and back of the glass substrate, with a screen printing speed of 250 mm / s, an ink return speed of 300 mm / s, and a screen printing pressure of 0.4 MPa, and baking and curing at 140° C. for 6 min to form an acid-resistant protective ink layer on the camera hole position on the front side of the glass substrate and the entire area on the back side;
[0036] (4) Immerse the glass substrate with the acid-resistant protective ink layer printed on it in an etching solution, wherein the etching solution comprises, by mass percentage, 22% ammonium hydrofluoride, 12% oxalic acid, 17% ammonium sulfate, 21% barium sulfate, 8% glycerol, and the remainder water, and etch at 35° C. for 1.5 min. After taking it out, rinse it with clean water, and etch the AG effect in the area of the glass substrate not covered by the acid-resistant ink layer;
[0037] (5) soaking the glass substrate etched with the AG effect in a deplating solution, wherein the deplating solution is a sodium hydroxide solution with a concentration of 8 wt %, soaking for 5 min at 60° C., then ultrasonically cleaning with deionized water, and drying;
[0038] (6) A spray gun is used to spray the hydrophobic coating onto the front surface of the glass substrate. The spraying rate is 3 m / s. The nozzle diameter of the spray gun is 1 mm. The distance between the nozzle and the surface of the glass substrate is 15 cm. The angle between the spray gun and the surface of the glass substrate is 50°. The hydrophobic coating comprises, by mass percentage, 18% of fluorinated modified organic silica sol, 12% of polytetrafluoroethylene powder (average particle size of 15 μm), 0.8% of BYK-333 leveling agent, and the balance is ethanol. The fluorinated modified organic silica sol is prepared by the following method: adding tetraethyl orthosilicate and tridecafluorooctyl triethoxysilane in a molar ratio of 1:0.2 to anhydrous ethanol to completely dissolve, and then adding nitric acid aqueous solution, the amount of nitric acid used is 1.2 times the molar amount of tetraethyl orthosilicate, heating to 60°C, stirring for reaction for 2 hours, and drying to obtain the fluorinated modified organic silica sol, and finally forming a hydrophobic layer on the front surface of the glass substrate.
[0039] The results of the AG glass obtained above show that the surface flatness of the camera hole area on the front side of the glass substrate is high, and the other areas except the camera hole area form an AG effect.
[0040] Example 2
[0041] This embodiment provides an etching method for AG glass, and the preparation method includes the following steps:
[0042] (1) providing a transparent glass substrate, ultrasonically cleaning the glass substrate with acetone and ethanol for 5 minutes in sequence, then rinsing it with deionized water, and drying it for later use;
[0043] (2) manufacturing a first film and a second film according to the outer dimensions of the front and back surfaces of the glass substrate, wherein the first film has a light-transmitting hole corresponding to the camera hole position on the front surface of the glass substrate and having a size 0.5 mm larger;
[0044] (3) The first film and the second film are exposed to light through a silk screen to produce a first printing screen and a second printing screen respectively, wherein only hollows corresponding to the light-transmitting holes are left on the first screen;
[0045] (3) using a first printing screen and a second printing screen to respectively screen-print the acid-resistant protective ink R568 on the front and back of the glass substrate, with a screen printing speed of 150 mm / s, an ink return speed of 400 mm / s, and a screen printing pressure of 0.3 MPa, and baking and curing at 150° C. for 5 min, so that an acid-resistant protective ink layer is formed on the camera hole position on the front side of the glass substrate and the entire area on the back side;
[0046] (4) Immerse the glass substrate with the acid-resistant protective ink layer printed on it in an etching solution, wherein the etching solution comprises, by mass percentage, 25% ammonium hydrofluoride, 10% oxalic acid, 20% ammonium sulfate, 20% barium sulfate, 10% glycerol, and the balance water, and etch at 30° C. for 2 min. After taking it out, rinse it with clean water, and etch the AG effect in the area of the glass substrate not covered by the acid-resistant ink layer;
[0047] (5) soaking the glass substrate etched with the AG effect in a deplating solution, wherein the deplating solution is a 10 wt % potassium hydroxide solution, soaking for 3 min at 80° C., then ultrasonically cleaning with deionized water, and drying;
[0048] (6) A spray gun is used to spray the hydrophobic coating onto the front surface of the glass substrate. The spraying rate is 2 m / s. The nozzle diameter of the spray gun is 2 mm. The distance between the nozzle and the surface of the glass substrate is 10 cm. The angle between the spray gun and the surface of the glass substrate is 50°. The hydrophobic coating comprises, by mass percentage, 15% of fluorinated modified organic silica sol, 15% of polytetrafluoroethylene powder (average particle size of 15 μm), 0.5% of BYK-333 leveling agent, and the balance is ethanol. The fluorinated modified organic silica sol is prepared by the following method: adding tetraethyl orthosilicate and tridecafluorooctyl triethoxysilane in a molar ratio of 1:0.2 to anhydrous ethanol to completely dissolve, and then adding nitric acid aqueous solution, the amount of nitric acid used is 1.2 times the molar amount of tetraethyl orthosilicate, heating to 60°C, stirring for reaction for 2 hours, and drying to obtain the fluorinated modified organic silica sol, and finally forming a hydrophobic layer on the front surface of the glass substrate.
[0049] The results of the AG glass obtained above show that the surface flatness of the camera hole area on the front side of the glass substrate is high, and the other areas except the camera hole area form an AG effect.
[0050] Example 3
[0051] This embodiment provides an etching method for AG glass, and the preparation method includes the following steps:
[0052] (1) providing a transparent glass substrate, ultrasonically cleaning the glass substrate with acetone and ethanol for 5 minutes in sequence, then rinsing it with deionized water, and drying it for later use;
[0053] (2) manufacturing a first film and a second film according to the outer dimensions of the front and back surfaces of the glass substrate, wherein the first film has a light-transmitting hole corresponding to the camera hole position on the front surface of the glass substrate and having a size 2 mm larger;
[0054] (3) The first film and the second film are exposed to light through a silk screen to produce a first printing screen and a second printing screen respectively, wherein only hollows corresponding to the light-transmitting holes are left on the first screen;
[0055] (3) using a first printing screen and a second printing screen to respectively screen print the acid-resistant protective ink R568 on the front and back of the glass substrate, with a screen printing speed of 350 mm / s, an ink return speed of 200 mm / s, and a screen printing pressure of 0.5 MPa, and baking and curing at 120° C. for 8 min to form an acid-resistant protective ink layer on the front camera hole position and the entire back area of the glass substrate;
[0056] (4) Immerse the glass substrate with the acid-resistant protective ink layer printed on it in an etching solution, wherein the etching solution comprises, by mass percentage, 20% ammonium hydrofluoride, 15% oxalic acid, 15% ammonium sulfate, 25% barium sulfate, 5% glycerol, and the balance water, and etch at 40° C. for 1 min. After taking it out, rinse it with clean water, and etch the AG effect in the area of the glass substrate not covered by the acid-resistant ink layer;
[0057] (5) soaking the glass substrate etched with the AG effect in a deplating solution, wherein the deplating solution is a 5 wt % sodium hydroxide solution, soaking for 8 min at 50° C., then ultrasonically cleaning with deionized water, and drying;
[0058] (6) A spray gun is used to spray the hydrophobic coating onto the front surface of the glass substrate. The spraying rate is 4 m / s. The nozzle diameter of the spray gun is 0.5 mm. The distance between the nozzle and the surface of the glass substrate is 20 cm. The angle between the spray gun and the surface of the glass substrate is 50°. The hydrophobic coating comprises, by mass percentage: 20% of fluorinated modified organic silica sol, 10% of polytetrafluoroethylene powder (average particle size of 15 μm), 1% of BYK-333 leveling agent, and the balance is ethanol. The fluorinated modified organic silica sol is prepared by the following method: tetraethyl orthosilicate and tridecafluorooctyl triethoxysilane are added to anhydrous ethanol in a molar ratio of 1:0.2 to completely dissolve, and then a nitric acid aqueous solution is added. The amount of nitric acid is 1.2 times the molar amount of tetraethyl orthosilicate. The temperature is raised to 60°C, stirred for reaction for 2 hours, and dried to obtain the fluorinated modified organic silica sol, and finally a hydrophobic layer is formed on the front surface of the glass substrate.
[0059] The results of the AG glass obtained above show that the surface flatness of the camera hole area on the front side of the glass substrate is high, and the other areas except the camera hole area form an AG effect.
[0060] Comparative Example 1
[0061] This comparative example proposes an etching method for AG glass, and the preparation method thereof comprises the following steps:
[0062] (1) providing a transparent glass substrate, ultrasonically cleaning the glass substrate with acetone and ethanol for 5 minutes in sequence, then rinsing it with deionized water, and drying it for later use;
[0063] (2) manufacturing a first film and a second film according to the outer dimensions of the front and back surfaces of the glass substrate, wherein the first film has a light-transmitting hole corresponding to the camera hole position on the front surface of the glass substrate and having a size 1 mm larger;
[0064] (3) The first film and the second film are exposed to light through a silk screen to produce a first printing screen and a second printing screen respectively, wherein only hollows corresponding to the light-transmitting holes are left on the first screen;
[0065] (3) using a first printing screen and a second printing screen to respectively screen-print the acid-resistant protective ink R568 on the front and back of the glass substrate, with a screen printing speed of 250 mm / s, an ink return speed of 300 mm / s, and a screen printing pressure of 0.4 MPa, and baking and curing at 140° C. for 6 min to form an acid-resistant protective ink layer on the camera hole position on the front side of the glass substrate and the entire area on the back side;
[0066] (4) Immerse the glass substrate with the acid-resistant protective ink layer printed on it in an etching solution, wherein the etching solution comprises, by mass percentage, 22% ammonium hydrofluoride, 12% oxalic acid, 17% ammonium sulfate, 21% barium sulfate, 8% glycerol, and the remainder water, and etch at 35° C. for 1.5 min. After taking it out, rinse it with clean water, and etch the AG effect in the area of the glass substrate not covered by the acid-resistant ink layer;
[0067] (5) soaking the glass substrate etched with the AG effect in a deplating solution, wherein the deplating solution is a sodium hydroxide solution with a concentration of 8 wt %, soaking for 5 min at 60° C., then ultrasonically cleaning with deionized water, and drying;
[0068] (6) A spray gun is used to spray the hydrophobic coating onto the front side of the glass substrate. The spraying rate is 3 m / s. The nozzle diameter of the spray gun is 1 mm. The distance between the nozzle and the surface of the glass substrate is 15 cm. The angle between the spray gun and the surface of the glass substrate is 50°. The hydrophobic coating comprises, by mass percentage, 18% of organic silica sol, 12% of polytetrafluoroethylene powder (with an average particle size of 15 μm), 0.8% of BYK-333 leveling agent, and the balance is ethanol. The organic silica sol is prepared by the following method: adding tetraethyl orthosilicate to anhydrous ethanol and dissolving it completely, then adding nitric acid aqueous solution, the amount of nitric acid being 1.2 times the molar amount of tetraethyl orthosilicate, heating to 60°C, stirring for reaction for 2 hours, and drying to obtain the organic silica sol, and finally forming a hydrophobic layer on the front side of the glass substrate.
[0069] The water contact angle of the AG glass obtained in the embodiment and the comparative example was measured using a contact angle meter, and the obtained AG glass was rubbed on 600-grit sandpaper to measure the water contact angle after rubbing 100 times. The structure is shown in Table 1 below.
[0070] Table 1 Hydrophobic properties of AG glass obtained in Examples and Comparative Examples
[0071]
[0072]
[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An etching method for AG glass, characterized in that: The steps include: S1, manufacturing the first and second films according to the external dimensions of the front and back surfaces of the glass substrate, wherein the first film also has a light-transmitting hole corresponding to the camera hole position on the front surface of the glass substrate; S2, making a printing screen according to the first and second films, and using the printing screen to screen print an acid-resistant protective ink layer on the camera hole position on the front side of the glass substrate and the entire area on the back side; S3, immersing the glass substrate with the acid-resistant protective ink layer printed on it in the etching solution, and etching the area on the glass substrate not covered by the acid-resistant ink layer to produce an AG effect; S4. Immerse the glass substrate etched with the AG effect in a deplating solution to remove the acid-resistant ink layer on the glass substrate.
2. The etching method of AG glass according to claim 1, characterized in that: The size of the light-transmitting hole on the first film is 0.05-2mm larger than the camera hole.
3. The etching method of AG glass according to claim 1 or 2, characterized in that: The thickness of the acid-resistant protective ink layer is 15-25 μm; Preferably, the screen printing rate is 150-350 mm / s, the ink return rate is 200-400 mm / s, and the screen printing pressure is 0.3-0.5 MPa.
4. The etching method of AG glass according to any one of claims 1 to 3, characterized in that: The acid-resistant ink layer is formed by curing at 120-150° C. for 5-8 minutes.
5. The etching method of AG glass according to any one of claims 1 to 4, characterized in that: The etching solution comprises, by mass percentage, 20-25% of ammonium hydrofluoride, 10-15% of oxalic acid, 15-20% of ammonium sulfate, 20-25% of barium sulfate, 5-10% of glycerol, and the balance of water.
6. The etching method of AG glass according to any one of claims 1 to 5, characterized in that: The etching temperature is 30-40° C. and the etching time is 1-2 minutes.
7. The etching method of AG glass according to any one of claims 1 to 6, characterized in that: The deplating solution is a sodium hydroxide or potassium hydroxide solution; Preferably, the concentration of the sodium hydroxide or potassium hydroxide solution is 5-10 wt %.
8. The etching method of AG glass according to any one of claims 1 to 7, characterized in that: After step S4, the method further includes: spraying a hydrophobic coating on the front side of the glass substrate to form a hydrophobic layer on the front side of the glass substrate.
9. The etching method of AG glass according to any one of claims 1 to 8, characterized in that: The hydrophobic coating comprises, by mass percentage, 15-20% of fluorinated modified organic silica sol, 10-15% of polytetrafluoroethylene powder, 0.5-1% of leveling agent, and the balance is ethanol.
10. An AG glass, characterized in that: The invention is prepared by the processing method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for energy-saving anti-icing / deicing coating combining super-hydrophobic coating and heating coating
CN105032731A
Glass etching technique
CN107804976A
Glass etching process
CN108545953A
Hydrophobic and oleophobic foam ceramic filter and preparation method thereof
CN110143809A
Processing method for avoiding camera hole site of display panel
CN112174539A