SAC overlay asphalt mixture as well as preparation and application thereof

By adding waste rubber-PE plastic composite modifier and basalt rock to the asphalt mixture, the high-temperature performance and low-temperature crack resistance of the asphalt pavement are improved, and the problem of easy cracking of asphalt pavement in the northwest plateau area is solved, and the pavement life is extended. Reduced construction and environmental impact.

CN118908630APending Publication Date: 2024-11-08GANSU TRANSPORTATION INVESTMENT MANAGEMENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972291.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the extreme climate of the northwest plateau area in my country, asphalt pavement is prone to cracking, loosening and other diseases, resulting in a reduction in surface life and complex natural conditions affecting the highway infrastructure, and comprehensive performance needs to be improved.

Method used

SAC cover asphalt mixture, including high viscosity asphalt, waste rubber-PE plastic composite modifier and graded aggregate, is prepared through specific heating and stirring processes, and waste rubber-PE plastic composite modifier is added to enhance the viscosity. For junction performance and flexibility, basalt rock material is used as grading aggregate to optimize particle size distribution.

Benefits of technology

It significantly improves high-temperature performance, low-temperature crack resistance and water stability, reduces construction difficulty and resource consumption, extends the road life, and improves environmental friendliness through energy conservation and emission reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the field of road asphalt mixtures, in particular to an SAC overlay asphalt mixture and preparation and application thereof.The SAC overlay asphalt mixture is prepared from asphalt, a waste rubber-PE plastic composite modifier and graded aggregate, the mass ratio of the asphalt to the waste rubber-PE plastic composite modifier is 1: (0.1-0.2), and the graded aggregate is prepared from the SAC overlay asphalt mixture, the waste rubber-PE plastic composite modifier and the graded aggregate. The ratio of the mass sum of the asphalt and the waste rubber-PE plastic composite modifier to the mass of the graded aggregate is (0.05-0.1): 1. Compared with the prior art, the adhesive has the advantages that the adhesive property is greatly improved, additives are easy to add, the construction difficulty is low and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of road asphalt mixtures, in particular to a SAC overlay asphalt mixture and the preparation and application thereof. Background Art

[0002] In the northwest plateau of my country, the climate is dry, the temperature difference between seasons is large, the temperature difference between day and night is large (-33.3℃-40℃), the temperature changes quickly, and the radiation during the day is extremely strong. Extreme climates such as large temperature differences and strong radiation can easily cause asphalt pavement cracking, rutting, loosening and other diseases. The appearance of these diseases greatly reduces the life of the asphalt surface layer. At the same time, complex natural conditions also have a great impact on infrastructure such as highway pavements. Asphalt pavement diseases occur frequently, and its comprehensive performance needs to be improved. Summary of the invention

[0003] The purpose of the present invention is to provide a SAC overlay asphalt mixture and its preparation and application in order to overcome the defects of the above-mentioned prior art.

[0004] The purpose of the present invention can be achieved by the following technical solutions:

[0005] A SAC overlay asphalt mixture, comprising: asphalt, waste rubber-PE plastic composite modifier and graded aggregate,

[0006] The mass ratio of the asphalt to the waste rubber-PE plastic composite modifier is 1:0.1-0.2, and the mass ratio of the sum of the mass of the asphalt and the waste rubber-PE plastic composite modifier to the graded aggregate is 0.05-0.1:1.

[0007] Furthermore, the asphalt is high-viscosity asphalt, and the viscosity of the high-viscosity asphalt is >20000 Pa·s.

[0008] Furthermore, the preparation process of the waste rubber-PE plastic composite modifier includes: shear mixing polyethylene and 90-110 mesh waste tire rubber powder at 160-180°C, post-drying, taking out and adding aromatic oil to stir and mix, post-drying and cooling to obtain the waste rubber-PE plastic composite modifier.

[0009] Furthermore, the composition of the graded aggregate is basalt stone, wherein the aggregate particle size distribution is:

[0010] The pass rate of aggregate corresponding to 0.075mm sieve holes is 4-6%, the pass rate of aggregate corresponding to 0.15mm sieve holes is 6-8%, the pass rate of aggregate corresponding to 0.3mm sieve holes is 8.5-11.5%, the pass rate of aggregate corresponding to 0.6mm sieve holes is 12-14%, the pass rate of aggregate corresponding to 1.18mm sieve holes is 16-18%, the pass rate of aggregate corresponding to 2.36mm sieve holes is 28-34%, the pass rate of aggregate corresponding to 4.75mm sieve holes is 45-65%, the pass rate of aggregate corresponding to 9.5mm sieve holes is 70-80%, the pass rate of aggregate corresponding to 13.2mm sieve holes is 85-95%, and the pass rate of aggregate corresponding to 16mm sieve holes is 98-100%.

[0011] A method for preparing a SAC overlay asphalt mixture, comprising:

[0012] The asphalt is heated and melted, and the graded aggregate is heated and dried. The dried graded aggregate is then initially stirred, and then the asphalt and the waste rubber-PE plastic composite modifier are added and mixed and stirred. After the stirring is completed, the SAC overlay asphalt mixture is obtained by discharging the material.

[0013] Furthermore, the heating and melting temperature is 160-170°C.

[0014] Furthermore, the heating and drying temperature is 175-185° C., and the heating and drying time is 4-6 hours.

[0015] Furthermore, the initial stirring time is 40-50s and the temperature is 180-190°C.

[0016] Furthermore, the mixing and stirring time is 80-90s and the temperature is 180-190°C.

[0017] Furthermore, the asphalt-to-stone ratio of the SAC overlay asphalt mixture is 4.0-5.5%.

[0018] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0019] 1) The rubber-plastic composite high-elasticity and crack-resistant ultra-thin overlay technology adopts the method of directly adding waste rubber-PE plastic composite modifiers. The waste rubber-PE plastic composite modifiers are directly added during the mixing process of the mixture, melted and dispersed under the high temperature and shearing action generated by mixing, which can greatly improve the bonding performance of the mixture. After the mixture is cooled, it can play a reinforcing role and improve the flexibility of the surface mixture. It successfully solves the disadvantage of the previous ultra-thin overlay technology that special modified asphalt must be used, and the operation is convenient and fast. The performance of asphalt and asphalt mixtures after adding waste rubber-PE plastic composite modifiers has been significantly improved. The high-temperature performance dynamic stability has increased by 62.5%; the low-temperature crack resistance has increased by 35%; the water stability has increased by 25%, and the performance of the pavement has been comprehensively improved, and the pavement life is estimated to be extended by 2 to 3 years.

[0020] 2) The asphalt pavement material of the present invention also has a relatively low construction difficulty, which makes the requirements for the mixing, paving and rolling of the mixture relatively low, thus making it more conducive for on-site construction personnel to effectively control the construction quality. At the same time, the ultra-thin overlay technology effectively saves non-renewable resources such as crushed stone and asphalt. 2 The road saves about 0.11 tons of asphalt mixture. It has significant energy-saving and emission-reduction effects in production, transportation, paving, rolling and other links. 2 The carbon emissions of roads in the five stages of asphalt mixture production, mixture mixing, transportation, paving and rolling were reduced by 4.6 tons, providing more favorable conditions for the widespread promotion and application of ultra-thin covering technology. DETAILED DESCRIPTION

[0021] The present invention is described in detail below with reference to specific embodiments.

[0022] A SAC overlay asphalt mixture, comprising: asphalt, waste rubber-PE plastic composite modifier and graded aggregate,

[0023] Among them, the mass ratio of the asphalt to the waste rubber-PE plastic composite modifier is 1:0.1-0.2, preferably 0.11:1, and the mass ratio of the sum of the mass of the asphalt and the waste rubber-PE plastic composite modifier to the graded aggregate is 0.05-0.1:1, preferably 0.05:1.

[0024] In some specific embodiments, the asphalt is high-viscosity asphalt, and the viscosity of the high-viscosity asphalt is >20000 Pa·s.

[0025] In some specific embodiments, the component of the graded aggregate is basalt stone, and in this graded aggregate, basalt stone is mainly included. The "mainly includes" here means that, first of all, the composition of the component graded aggregate is basically composed of basalt stone. The so-called "basically composed of basalt stone" means that in the case of unavoidable impurities, the main body of the component graded aggregate is composed of basalt stone. Secondly, the component graded aggregate may also contain a certain proportion of main basalt stone as the main aggregate, and a small amount of filler or other secondary aggregate may be added. In this case, technicians in the professional field can understand that the core component of the aggregate is mainly basalt stone. Preferably, basalt stone accounts for more than 90% of the weight of the aggregate, and even more preferably more than 95%.

[0026] Among them, the particle size distribution of aggregate is:

[0027] The pass rate of aggregate corresponding to 0.075mm sieve holes is 4-6%, the pass rate of aggregate corresponding to 0.15mm sieve holes is 6-8%, the pass rate of aggregate corresponding to 0.3mm sieve holes is 8.5-11.5%, the pass rate of aggregate corresponding to 0.6mm sieve holes is 12-14%, the pass rate of aggregate corresponding to 1.18mm sieve holes is 16-18%, the pass rate of aggregate corresponding to 2.36mm sieve holes is 28-34%, the pass rate of aggregate corresponding to 4.75mm sieve holes is 45-65%, the pass rate of aggregate corresponding to 9.5mm sieve holes is 70-80%, the pass rate of aggregate corresponding to 13.2mm sieve holes is 85-95%, and the pass rate of aggregate corresponding to 16mm sieve holes is 98-100%.

[0028] A method for preparing a SAC overlay asphalt mixture, comprising:

[0029] The asphalt is heated and melted, and the graded aggregate is heated and dried. The dried graded aggregate is then initially stirred, and then the asphalt and the waste rubber-PE plastic composite modifier are added and mixed and stirred. After the stirring is completed, the SAC overlay asphalt mixture is obtained by discharging the material.

[0030] In some specific embodiments, the heating and melting temperature is 160-170°C, preferably 170°C, and the heating is performed for 2 hours.

[0031] In some specific embodiments, the heating and drying temperature is 175-185° C., and the heating and drying time is 4-6 hours, preferably drying at 180° C. for 5 hours.

[0032] In some specific embodiments, the initial stirring time is 40-50 s and the temperature is 180-190°C, preferably the stirring time is 45 s and the stirring temperature is 185°C.

[0033] In some specific embodiments, the mixing and stirring time is 80-90 seconds and the temperature is 180-190°C, preferably the mixing time is 90 seconds and the mixing temperature is 185°C.

[0034] In some specific embodiments, the asphalt-to-stone ratio of the SAC overlay asphalt mixture is 4.0-5.5%.

[0035] In the following embodiments, the preparation process of the waste rubber-PE plastic composite modifier is as follows: low-density polyethylene and 100-mesh waste tire rubber powder are sheared and mixed at a mass ratio of 1:5 at 170°C by a high-speed shearing machine at a speed of 3000 rpm, and the finished product is placed in an oven after the shearing is completed, and is kept warm at 110°C for 1 hour, and then taken out and mixed with asphalt modified special aromatic oil at a mass ratio of 1:20, and the rubber-plastic composite is mixed with the aromatic oil by a low-speed mixer at a speed of 500 rpm, and the finished product is placed in an oven after the stirring is completed, and is kept warm at 110°C for 1 hour. Then take it out and cool it naturally, and shear the solid mixture into solid particles with a diameter of 0.8 mm for standby use.

[0036] In the following examples, the main physical indicators of the waste rubber-PE plastic composite modifier are

[0037] Table 1 Main physical indicators of waste rubber-PE plastic composite modifier

[0038]

[0039] In the following examples, asphalt: domestic high-viscosity asphalt, which is currently widely used in porous asphalt pavements, and its technical indicators meet the technical requirements of "Technical Specifications for Highway Asphalt Pavement Construction" JTGF40-2004;

[0040] Limestone powder: The powder obtained by grinding limestone, the technical indicators of which meet the technical requirements of "Technical Specifications for Highway Asphalt Pavement Construction" JTGF40-2004;

[0041] Aggregate: The main component is basalt aggregate, which is also mixed with some mineral powder. The gradation of basalt aggregate is shown in Table 2. The gradation range reflects the particle size of the aggregate used and its proportion.

[0042] Table 2 Pass rate of basalt aggregate of various particle sizes

[0043]

[0044]

[0045] In the following examples, asphalt mixtures were prepared according to 1 volume part of domestic high-viscosity asphalt, 0.11 volume parts of waste rubber-PE plastic composite modifier, and 4.5 wt% of asphalt-stone ratio, and the mixtures were prepared according to the "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011).

[0046] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0047] The following are more detailed implementation cases, which further illustrate the technical solutions of the present invention and the technical effects that can be obtained.

[0048] Example 1

[0049] This embodiment provides a SAC overlay asphalt mixture and a preparation method thereof, comprising:

[0050] 1) Place 11.52 kg of graded aggregate in an oven and heat and dry it at 180°C for 5 hours for later use; Place 1.5 kg of asphalt in an oven and heat and melt it at 170°C for 2 hours for later use;

[0051] 2) Take 60.31g of waste rubber-PE plastic composite modifier, 518.40g of fully heated asphalt, and 11520g of graded aggregate (basalt aggregate + mineral powder);

[0052] 3) First, put the graded aggregate into a stirring pot and heat it at 180℃ for 45s;

[0053] 4) Then, add asphalt and waste rubber-PE plastic composite modifier into the stirring pot and heat at 180°C for 90s;

[0054] 5) Discharge after mixing is completed.

[0055] The graded aggregate in this embodiment has a graded composition as shown in Table 3.

[0056] Table 3 Aggregate gradation composition design of Example 1

[0057]

[0058]

[0059] Comparative Example 1

[0060] This comparative example provides an asphalt mixture, which is different from Example 1 in that:

[0061] In step 2), no waste rubber-PE plastic composite modifier is added, and the other steps are the same as in Example 1.

[0062] The two mixtures obtained in Example 1 and Comparative Example 1 were subjected to the Marshall stability test for asphalt mixture immersion (T0709-2011), the freeze-thaw splitting test for asphalt mixture (T0729-2000), and the Kentenberg dispersion test for asphalt mixture (T0733-2011) in accordance with the requirements of JTG E20-2011 "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering". The test results and the required values ​​of the specification are shown in Tables 4-5.

[0063] Table 4 Road performance test results of Example 1

[0064]

[0065] Table 5 Comparative Example 1 Related Road Performance Test Results

[0066]

[0067] Example 2

[0068] This embodiment provides an ultra-thin overlay asphalt concrete, which is prepared by the following steps:

[0069] Steps 1), 3), 4), and 5) are the same as in Example 1;

[0070] Step 2): Take 57.6g of waste rubber-PE plastic composite modifier, 495.36g of fully heated asphalt, and 11520g of graded aggregate;

[0071] For the aggregate described in 1), its gradation composition is shown in Table 6

[0072] Table 6 Aggregate gradation composition design of Example 2

[0073]

[0074]

[0075] Comparative Example 2

[0076] This comparative example provides an asphalt mixture, which is different from Example 2 in that:

[0077] In step 2), no waste rubber-PE plastic composite modifier is added, and the other steps are the same as in Example 2.

[0078] The two mixtures obtained in Example 2 and Comparative Example 2 were subjected to the Marshall stability test for asphalt mixture immersion (T0709-2011), the freeze-thaw splitting test for asphalt mixture (T0729-2000), and the Kentenberg dispersion test for asphalt mixture (T0733-2011) in accordance with the requirements of JTG E20-2011 "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering". The test results and the required values ​​of the specification are shown in Tables 7 and 8.

[0079] Table 7 Road performance test results of Example 2

[0080]

[0081] Table 8 Comparative Example 2 Related Road Performance Test Results

[0082]

[0083] Combining the road performance test results of the asphalt mixture prepared with the high-viscosity asphalt used in Examples 1 and 2, it can be seen that the asphalt mixture added with the waste rubber-PE plastic composite modifier has high durability, anti-scattering and spalling performance and water stability.

[0084] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A SAC overlay asphalt mixture, characterized in that: include: Asphalt, waste rubber-PE plastic composite modifier and graded aggregate, The mass ratio of the asphalt to the waste rubber-PE plastic composite modifier is 1:0.1-0.2, and the mass ratio of the sum of the mass of the asphalt and the waste rubber-PE plastic composite modifier to the graded aggregate is 0.05-0.1:

1.

2. The SAC overlay asphalt mixture according to claim 1, characterized in that: The asphalt is high-viscosity asphalt, and the viscosity of the high-viscosity asphalt is greater than 20000 Pa·s.

3. The SAC overlay asphalt mixture according to claim 1, characterized in that: The preparation process of the waste rubber-PE plastic composite modifier comprises: shearing and mixing polyethylene and 90-110 mesh waste tire rubber powder at 160-180° C., drying, taking out, adding aromatic oil, stirring and mixing, and drying and cooling to obtain the waste rubber-PE plastic composite modifier.

4. The SAC overlay asphalt mixture according to claim 1, characterized in that: The composition of the graded aggregate is basalt stone, wherein the particle size distribution of the aggregate is: The pass rate of aggregate corresponding to 0.075mm sieve holes is 4-6%, the pass rate of aggregate corresponding to 0.15mm sieve holes is 6-8%, the pass rate of aggregate corresponding to 0.3mm sieve holes is 8.5-11.5%, the pass rate of aggregate corresponding to 0.6mm sieve holes is 12-14%, the pass rate of aggregate corresponding to 1.18mm sieve holes is 16-18%, the pass rate of aggregate corresponding to 2.36mm sieve holes is 28-34%, the pass rate of aggregate corresponding to 4.75mm sieve holes is 45-65%, the pass rate of aggregate corresponding to 9.5mm sieve holes is 70-80%, the pass rate of aggregate corresponding to 13.2mm sieve holes is 85-95%, and the pass rate of aggregate corresponding to 16mm sieve holes is 98-100%.

5. A method for preparing a SAC overlay asphalt mixture as claimed in any one of claims 1 to 4, characterized in that: include: The asphalt is heated and melted, and the graded aggregate is heated and dried. The dried graded aggregate is then initially stirred, and then the asphalt and the waste rubber-PE plastic composite modifier are added and mixed and stirred. After the stirring is completed, the SAC overlay asphalt mixture is obtained by discharging the material.

6. The method for preparing the SAC overlay asphalt mixture according to claim 5, characterized in that: The heating and melting temperature is 160-170°C.

7. The method for preparing the SAC overlay asphalt mixture according to claim 5, characterized in that: The heating and drying temperature is 175-185° C., and the heating and drying time is 4-6 hours.

8. The method for preparing the SAC overlay asphalt mixture according to claim 5, characterized in that: The initial stirring time is 40-50 seconds and the temperature is 180-190°C.

9. The method for preparing the SAC overlay asphalt mixture according to claim 5, characterized in that: The mixing and stirring time is 80-90s, and the temperature is 180-190°C.

10. The method for preparing the SAC overlay asphalt mixture according to claim 5, characterized in that: The asphalt-to-stone ratio of the SAC overlay asphalt mixture is 4.0-5.5%.