Composite self-healing waterproof agent and preparation method thereof

By using polyvinyl alcohol-encapsulated open-hole glass microbeads and permeable crystal masterbatch in the waterproofing agent, a composite self-healing waterproofing agent is formed, which solves the problem of poor adhesion of the waterproof layer, and achieves efficient waterproofing effect and construction convenience. Reduced costs.

CN118908654APending Publication Date: 2024-11-08福建省三棵树新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410965417.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing waterproofing agents have poor adhesion when the water-based inorganic materials are combined with oily asphalt-based materials, resulting in cracking, leaking and hollowing of the waterproof layer, and long construction time and high cost.

Method used

Open-porous hollow glass microbeads wrapped with polyvinyl alcohol and permeable crystal masterbatch form a composite self-healing waterproofing agent. After absorbing water, polyvinyl alcohol forms a gel-like substance and bonds to the asphalt coil, and fills the gaps through permeable crystal expansion. , improve adhesion and waterproofing.

Benefits of technology

Effectively prevent hollowing, seepage, and water splashing problems in the construction of wet waterproof rolls, improve waterproofing grade, reduce construction time and cost, improve interlayer adhesion, and significantly improve waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908654A_ABST
    Figure CN118908654A_ABST
Patent Text Reader

Abstract

The invention relates to a composite self-healing waterproof agent and a preparation method thereof. The composite self-healing waterproof agent is mainly prepared from the following components in parts by weight: 45 parts of Portland cement, 45 parts of quartz sand, 0.5-1 part of hollow glass beads, 1-2 parts of capillary crystalline master batch, 3-5 parts of polyvinyl alcohol, 0.2 part of a defoaming agent and 1.8-5.3 parts of heavy calcium carbonate. The composite self-healing waterproof agent disclosed by the invention can effectively prevent the problems of hollowing, water seepage and water leaping caused in the construction process of a wet-laid waterproof coiled material, the waterproof grade is improved, the interlayer cohesiveness of a waterproof coating layer is improved, the construction time is shortened, and the labor cost and the material cost are saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite self-healing waterproofing agent and a preparation method thereof, and is applied in the field of waterproofing agents. Background Art

[0002] With the gradual maturity of waterproofing agents and the increasing sales share, the market's strict requirements on waterproofing levels and the increase in demand for building waterproofing, there are more and more scenarios for the combined use of waterproofing agents and waterproof membranes. Therefore, in order to improve the poor composite adhesion between water-based inorganic materials and oily asphalt-based materials, cracking, leakage, and hollowing of the waterproof layer, this patent proposes a composite self-healing waterproofing agent and a preparation method to improve the waterproofing level, improve the interlayer adhesion of the waterproof coating, reduce construction time, and save labor costs. Summary of the invention

[0003] The present invention provides a composite self-healing waterproof agent and a preparation method thereof. The composite self-healing waterproof agent of the present invention can effectively prevent hollowing, water seepage and water leakage problems caused by wet-laid waterproof coiled materials during construction, improve the waterproof grade, improve the interlayer adhesion of the waterproof coating, reduce construction time, save labor costs, and save material costs.

[0004] The technical solution of the present invention is as follows:

[0005] A composite self-healing waterproofing agent is mainly prepared from the following components in the following weight ratios:

[0006] Based on the total weight of the material, the liquid material:

[0007]

[0008] The composite self-healing waterproofing agent of the present application optimizes the raw material formula and uses polyvinyl alcohol to wrap the hollow glass microspheres containing the infiltration crystallization masterbatch. After the material is formed, if there is a problem of water seepage or moisture, it will gradually absorb water and release it. First, the polyvinyl alcohol absorbs water and dissolves, forming a colloid in the gap and bonding with the surface of the asphalt coil. When it continues to encounter water, the infiltration crystallization masterbatch in the open-pored glass microspheres will absorb water to form crystals, which will slowly expand and fill the leaking gaps to achieve a water-stopping effect. During the construction of wet-laid asphalt coils, the composite self-healing waterproofing agent is evenly sprinkled on the surface of the cement slurry, and then the asphalt coil is pasted, which is convenient for construction.

[0009] The silicate cement is ordinary silicate cement with the grade of P.O42.5, which saves material cost and ensures that the product has higher strength.

[0010] The heavy calcium carbonate is heavy calcium carbonate powder with a mesh size of 200-300.

[0011] The dispersible latex powder is formed by copolymerization of styrene acrylate and is spray-dried to form a freely flowing white powder to ensure the waterproof property of the material itself.

[0012] The hollow glass microspheres are glass microspheres with a particle size of 75-100 microns;

[0013] The infiltration crystallization masterbatch is made of composite powder materials such as aluminum sulfate and magnesium sulfate with a mesh size of more than 300 meshes;

[0014] The polyvinyl alcohol is a white powder with a melting point of 150° C.-220° C.

[0015] The defoaming agent selected is Japan's Sannopco, which uses polyethylene glycol or polysiloxane powder defoaming agents suitable for alkaline media. It can effectively inhibit and eliminate bubbles during the construction process and ensure the waterproof performance of the material.

[0016] The preparation method of the composite self-healing waterproof agent comprises the following steps:

[0017] 1) Preparation of open-pore hollow glass microspheres: Add 0.5-1 parts of hollow glass microspheres to hydrofluoric acid, stir for 0.5-1h, filter, wash and dry to obtain open-pore hollow glass microspheres; add 10 mL of hydrofluoric acid for every 0.5-1 g of hollow glass microspheres.

[0018] 2) preparing filled glass microspheres: adding the open-pore hollow glass microspheres prepared in step 1) and 1-2 parts of the infiltration crystallization masterbatch into a container and turning and stirring the container in a sealed state for 4-5 hours to obtain filled glass microspheres;

[0019] 3) preparing polyvinyl alcohol-wrapped filled glass microspheres: adding the filled glass microspheres prepared in step 2) into a container, and spraying 3-5 parts of polyvinyl alcohol hot-melt at 100-140° C. onto the surface of the filled glass microspheres in the container under pressure at a stirring rate of 1000-1400 rpm, and then cooling naturally;

[0020] 4) Preparation of powder: Finally, 45 parts of silicate cement, 45 parts of quartz sand, 1.8-5.3 parts of heavy calcium carbonate, 0.2 parts of defoaming agent, and the polyvinyl alcohol-wrapped filling glass microspheres obtained in step 3) are mixed to obtain the composite self-healing waterproofing agent.

[0021] Step 2) After stirring for 4-5 hours, filter with a 250-300 mesh screen. If the sieved infiltration crystallization masterbatch is higher than 50% of the added amount, add the material back to the container and continue stirring until the sieved infiltration crystallization masterbatch is lower than 50% of the added amount, then stop stirring.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] By filling the open holes of hollow glass microspheres with penetrating crystallization waterproof masterbatch and wrapping the surface of the filled glass microspheres with polyvinyl alcohol, the material can gradually release the effective ingredients when it comes into contact with water, and fill and seal the seepage and leakage points. After absorbing water, polyvinyl alcohol can enhance the adhesion between cement-based materials and asphalt membranes and improve the interlayer bonding; at the same time, the various selected gel materials and additives ensure that the product has excellent mechanical properties, waterproof properties and cost advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the penetration effect of the material and the base concrete observed under the magnifying glass of Example 1. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is described in detail below in conjunction with embodiments.

[0026] Example 1

[0027] The composite self-healing waterproofing agent described in the present invention is prepared from the following components in parts by weight:

[0028]

[0029] The preparation method of the composite self-healing waterproof agent comprises the following steps:

[0030] 1) Preparation of open-pore hollow glass microspheres: adding hollow glass microspheres to 10 mL of hydrofluoric acid and stirring for 0.5 h, followed by filtering, washing, and drying to obtain open-pore hollow glass microspheres;

[0031] 2) preparing filled glass microspheres: adding the open-pore hollow glass microspheres prepared in step 1) and the infiltration crystallization masterbatch into a container and turning and stirring the container in a sealed state for 4 hours to obtain filled glass microspheres;

[0032] 3) preparing polyvinyl alcohol-wrapped filled glass microspheres: adding the filled glass microspheres prepared in step 2) into a container, and spraying 100° C. hot-melt polyvinyl alcohol under pressure onto the surface of the filled glass microspheres in the container at a stirring rate of 1000 rpm, and then cooling naturally;

[0033] 4) Preparing powder: Finally, silicate cement, quartz sand, heavy calcium carbonate, defoaming agent, and polyvinyl alcohol-wrapped glass microspheres prepared in step 3) are mixed to obtain the composite self-healing waterproofing agent.

[0034] Step 2) After stirring for 4 hours, filter with a 250-300 mesh sieve. If the sieved infiltration crystallization masterbatch is less than 50% of the added amount, stop stirring. Otherwise, continue stirring until the sieved infiltration crystallization masterbatch is less than 50% of the added amount.

[0035] Sprinkle the above materials dry on the cement slurry surface and then carry out wet-laying roll material construction.

[0036] Example 2

[0037] The composite self-healing waterproofing agent described in the present invention is prepared from the following components in parts by weight:

[0038]

[0039] The preparation method of the composite self-healing waterproof agent comprises the following steps:

[0040] 1) Preparation of open-pore hollow glass microspheres: adding hollow glass microspheres to 10 mL of hydrofluoric acid and stirring for 0.6 h, followed by filtering, washing, and drying to obtain open-pore hollow glass microspheres;

[0041] 2) preparing filled glass microspheres: adding the open-pore hollow glass microspheres prepared in step 1) and the infiltration crystallization masterbatch into a container and turning and stirring the container in a sealed state for 5 hours to obtain filled glass microspheres;

[0042] 3) Preparing polyvinyl alcohol-wrapped filled glass microspheres: adding the filled glass microspheres prepared in step 2) into a container, and spraying 140° C. hot-melt polyvinyl alcohol under pressure onto the surface of the filled glass microspheres in the container at a stirring rate of 1400 rpm, followed by natural cooling;

[0043] 4) Preparing powder: Finally, silicate cement, quartz sand, heavy calcium carbonate, defoaming agent, and polyvinyl alcohol-wrapped glass microspheres prepared in step 3) are mixed to obtain the composite self-healing waterproofing agent.

[0044] Step 2) After stirring for 5 hours, filter with a 250-300 mesh sieve. If the sieved infiltration crystallization masterbatch is less than 50% of the added amount, stop stirring. Otherwise, continue stirring until the sieved infiltration crystallization masterbatch is less than 50% of the added amount.

[0045] Sprinkle the above materials dry on the cement slurry surface and then carry out wet-laying roll material construction.

[0046] Example 3

[0047] The composite self-healing waterproofing agent described in the present invention is prepared from the following components in parts by weight:

[0048]

[0049]

[0050] The preparation method of the composite self-healing waterproof agent comprises the following steps:

[0051] 1) Preparation of open-pore hollow glass microspheres: adding hollow glass microspheres to 10 mL of hydrofluoric acid and stirring for 1 hour, followed by filtering, washing, and drying to obtain open-pore hollow glass microspheres;

[0052] 2) preparing filled glass microspheres: adding the open-pore hollow glass microspheres prepared in step 1) and the infiltration crystallization masterbatch into a container and turning and stirring the container in a sealed state for 4.5 hours to obtain filled glass microspheres;

[0053] 3) Preparing polyvinyl alcohol-wrapped filled glass microspheres: adding the filled glass microspheres prepared in step 2) into a container, and spraying 120° C. hot-melt polyvinyl alcohol under pressure onto the surface of the filled glass microspheres in the container at a stirring rate of 1200 rpm, followed by natural cooling;

[0054] 4) Preparing powder: Finally, silicate cement, quartz sand, heavy calcium carbonate, defoaming agent, and polyvinyl alcohol-wrapped glass microspheres prepared in step 3) are mixed to obtain the composite self-healing waterproofing agent.

[0055] Step 2) After stirring for 4.5 hours, filter with a 250-300 mesh sieve. If the sieved infiltration crystallization masterbatch is less than 50% of the added amount, stop stirring. Otherwise, continue stirring until the sieved infiltration crystallization masterbatch is less than 50% of the added amount.

[0056] Sprinkle the above materials dry on the cement slurry surface and then carry out wet-laying roll material construction.

[0057] Example 4

[0058] The composite self-healing waterproofing agent described in the present invention is prepared from the following components in parts by weight:

[0059]

[0060] The preparation method of the composite self-healing waterproof agent comprises the following steps:

[0061] 1) Preparation of open-pore hollow glass microspheres: adding hollow glass microspheres to 10 mL of hydrofluoric acid and stirring for 1 hour, followed by filtering, washing, and drying to obtain open-pore hollow glass microspheres;

[0062] 2) preparing filled glass microspheres: adding the open-pore hollow glass microspheres prepared in step 1) and the infiltration crystallization masterbatch into a container and turning and stirring the container in a sealed state for 4.5 hours to obtain filled glass microspheres;

[0063] 3) Preparing polyvinyl alcohol-wrapped filled glass microspheres: adding the filled glass microspheres prepared in step 2) into a container, and spraying 3-5 parts of polyvinyl alcohol hot-melt at 120° C. onto the surface of the filled glass microspheres in the container under pressure at a stirring rate of 1200 rpm, and then cooling naturally;

[0064] 4) Preparing powder: Finally, silicate cement, quartz sand, heavy calcium carbonate, defoaming agent, and polyvinyl alcohol-wrapped glass microspheres prepared in step 3) are mixed to obtain the composite self-healing waterproofing agent.

[0065] Step 2) After stirring for 4.5 hours, filter with a 250-300 mesh sieve. If the sieved infiltration crystallization masterbatch is less than 50% of the added amount, stop stirring. Otherwise, continue stirring until the sieved infiltration crystallization masterbatch is less than 50% of the added amount.

[0066] Sprinkle the above materials dry on the cement slurry surface and then carry out wet-laying roll material construction.

[0067] Comparative Example 1

[0068] This solution is used as a comparison to not add the material of the present invention, and directly carry out cement slurry bonding wet laying coiled material construction.

[0069] Comparative Example 2

[0070] This solution compares the waterproof effect and bonding effect with asphalt membrane of filled glass microspheres without adding polyvinyl alcohol. It is mainly prepared by the following components according to the weight ratio in the following table:

[0071]

[0072] The preparation method of the composite self-healing waterproofing agent filled with glass microspheres without adding vinyl alcohol treatment comprises the following steps:

[0073] Preparation of the material: Add the silicate cement, quartz sand, dispersible latex powder, defoamer and heavy calcium carbonate in sequence and mix them, dry-sprinkle them on the surface of cement slurry and then wet-lay the roll material for construction.

[0074] Performance test experimental data:

[0075] like Figure 1 The figure shows the penetration effect of the material and the base concrete under the magnifying glass of Example 1, where 1 is the waterproofing agent layer, and 2 and 3 are both bases. There is a crystallized penetrating waterproofing agent layer in the base of 2, and the base of 3 has not yet penetrated and crystallized.

[0076] The composite self-healing waterproofing agent of each embodiment was tested for indicators according to the test method of reference standard JCT 2090-2011 "Polymer Cement Waterproofing Slurry". The test results are shown in Table 1:

[0077] Table 1 Composite self-healing waterproofing agent performance test results

[0078]

[0079] It can be seen from Table 1 that the composite self-healing waterproofing agent has excellent mechanical properties (compressive and flexural strengths are higher than the reference standard), which can effectively prevent hollowing, water seepage, and water leakage caused by wet-laid waterproofing membranes during construction. When damage occurs, the material can effectively absorb water and swell to grow crystals to fill the leaks.

[0080] Raw material information:

[0081]

[0082] The defoaming agent is a powder defoaming agent of Japan Sannopco polyethylene glycol or polysiloxane suitable for alkaline media.

[0083] The present invention is not limited to the above embodiments. Any improvement or replacement based on the principle of the present invention should be within the protection scope of the present invention.

Claims

1. A composite self-healing waterproofing agent, Features: It is mainly prepared from the following components by weight:

2. The composite self-healing waterproofing agent according to claim 1, Features: The hollow glass microspheres are hollow glass microspheres with a particle size of 75-100 microns.

3. The composite self-healing waterproofing agent according to claim 1, Features: The infiltration crystallization masterbatch is aluminum sulfate powder or magnesium sulfate powder with a mesh size greater than 300 meshes.

4. The composite self-healing waterproofing agent according to claim 1, Features: The heavy calcium carbonate is heavy calcium carbonate powder with a mesh size of 200-300.

5. A method for preparing a composite self-healing waterproofing agent according to any one of claims 1 to 4, Features: The following steps are involved: 1) Preparation of open-pore hollow glass microspheres: adding 0.5-1 parts of hollow glass microspheres to hydrofluoric acid, stirring for 0.5-1h, filtering, washing, and drying to obtain open-pore hollow glass microspheres; adding 10 mL of hydrofluoric acid for every 0.5-1g of hollow glass microspheres; 2) preparing filled glass microspheres: adding the open-pore hollow glass microspheres prepared in step 1) and 1-2 parts of the infiltration crystallization masterbatch into a container and turning and stirring the container in a sealed state for 4-5 hours to obtain filled glass microspheres; 3) preparing polyvinyl alcohol-wrapped filled glass microspheres: adding the filled glass microspheres prepared in step 2) into a container, and spraying 3-5 parts of polyvinyl alcohol hot-melt at 100-140° C. onto the surface of the filled glass microspheres in the container under pressure at a stirring rate of 1000-1400 rpm, followed by natural cooling; 4) Preparation of powder: Finally, 45 parts of silicate cement, 45 parts of quartz sand, 1.8-5.3 parts of heavy calcium carbonate, 0.2 parts of defoaming agent, and the polyvinyl alcohol-wrapped filling glass microspheres obtained in step 3) are mixed to obtain the composite self-healing waterproofing agent.

6. The preparation method of the composite self-healing waterproofing agent according to claim 5, Features: Step 2) After stirring for 4-5 hours, filter with a 250-300 mesh screen. If the sieved infiltration crystallization masterbatch is higher than 50% of the added amount, add the material back to the container and continue stirring until the sieved infiltration crystallization masterbatch is lower than 50% of the added amount, then stop stirring.