Large-filling-amount steel slag roadbed filling material and preparation method thereof
By mixing and mixing steel slag, cement, fly ash and clay, efficient roadbed fill materials are prepared, which solves the problem that steel slag is difficult to form in roadbed fill, and improves the mechanical properties and regeneration of roadbed fills. The road construction has been achieved with economic and environmental protection.
Patent Information
- Application Number
- CN202411009175.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
Due to the lack of bonding effect, steel slag is difficult to form in roadbed fill, and it will reduce road performance after being added in large quantities. The existing research mainly focuses on the use of small amounts and the need for auxiliary materials to ensure material integrity.
By mixing and mixing steel slag, cement, fly ash and clay, steel slag with a total mass percentage of 40-65%, 1-4% cement, 5-10% fly ash, 10-18% The water and the remaining part are clay roadbed filler materials, and the uniformity and bonding effect of the material are ensured through jaw crushing, drying, air drying, stirring and stirring.
The effective recycling and utilization of large-filled steel slag has been achieved, the compressive strength and shear strength of roadbed fill has been improved, the freeze-thaw cycle damage has been reduced, the service period of the road has been extended, and construction costs and environmental pollution have been reduced.
Smart Images

Figure CN118908659A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of highway roadbed, and in particular relates to a large-volume steel slag roadbed filling material and a preparation method thereof. Background Art
[0002] Steel slag is called "resources in the wrong place". With the increase of industrial demand, the mining of iron ore has been increasing. A large amount of steel ore waste slag is produced during steelmaking. Since the iron content in the waste is low and it is difficult to use it for other purposes, a large amount of steel slag is piled up in the waste yard for a long time and cannot be effectively recycled. In addition, the large amount of accumulated waste not only occupies a large area of land, but also causes a lot of economic losses.
[0003] The use of industrial waste in roadbed construction is an important way to reduce the construction cost of roadbed fill and avoid the long-term accumulation of waste. However, industrial waste generally does not have a bonding effect, which leads to the inability to effectively shape the waste after it is added to the roadbed fill. In particular, large amounts of steel slag are more difficult to shape. After a small amount of steel slag is added to the roadbed fill, the road performance is greatly reduced. Therefore, adding a large amount of steel slag to the roadbed fill can greatly reduce waste accumulation and reduce the economic cost of the roadbed fill in the project. However, how to ensure the road performance strength of the roadbed is an important research content for the utilization of large amounts of waste.
[0004] There are some studies on industrial wastes such as steel slag, but only a small amount of steel slag, iron tailings and other industrial wastes are added to asphalt mixtures or roadbed fills. In addition, curing agents, fibers and other materials are needed to ensure the integrity of the materials. The actual construction methods and engineering materials for engineering applications have higher requirements. Whether industrial waste meets the requirements of road performance after being added to the roadbed fill is also the key to its application. Therefore, the engineering application of large amounts of steel slag must not only maintain good road performance, but also require simple construction and low process costs. In summary, the application of large amounts of industrial waste slag in infrastructure construction has good application prospects, but ensuring the strength of the material while using it in large quantities is a key issue that needs to be solved. Summary of the invention
[0005] The embodiment of the present invention provides a large-volume steel slag roadbed fill material and a preparation method thereof, which solves the problem that industrial waste generally has no bonding effect, resulting in the waste being unable to be effectively formed after being added to the roadbed fill, especially a large amount of steel slag is more difficult to form, and the road performance is greatly reduced after a small amount of steel slag is added to the roadbed fill.
[0006] In view of the above problems, the technical solution proposed by the present invention is:
[0007] The present invention provides a large-volume steel slag roadbed filling material and a preparation method thereof, comprising stirring and mixing steel slag, cement, fly ash, water and clay to obtain the roadbed filling material, wherein the total mass percentage of the roadbed filling material is 40-65% of steel slag, 1-4% of cement, 5-10% of fly ash, 10-18% of water, and the remainder is clay, wherein the preparation method of the roadbed filling material comprises the following steps:
[0008] S1, using a jaw crusher to crush steel slag and clay, drying them in the sun and air, passing the steel slag through a 20 mm soil sieve, crushing and sieving the sieved part again, and selecting the sieved part with a diameter less than 20 mm;
[0009] S2, when preparing in a mixing plant, dry steel slag, clay, cement, fly ash and water with the corresponding optimum moisture content are weighed according to the total mass percentage, firstly steel slag, clay, cement and fly ash with a size less than 20 mm are put into a mixer and stirred for 10-15 minutes, and then water with the optimum moisture content is added into the mixer and stirred for 10-15 minutes;
[0010] S3, when mixing on site, weigh dry steel slag, clay, cement, fly ash and water with the corresponding optimum moisture content according to the above total mass percentage, mix the steel slag, clay, cement and fly ash with a size less than 20 mm on site with a mixing machine, add water with a moisture content exceeding 2% of the optimum moisture content after mixing for 10-15 minutes, and continue mixing for 10-15 minutes;
[0011] S4, lay the mixed roadbed fill material on the roadbed in a normal layered paving manner, and after rolling and compaction to reach the specified compaction degree, cover the roadbed with a protective layer, complete the natural settlement of the roadbed and the steel slag roadbed fill maintenance for 7 days, and then set up other road structures.
[0012] As a preferred technical solution of the present invention, the type of the steel slag is massive steel slag after steelmaking.
[0013] As a preferred technical solution of the present invention, the type of cement is any one of ordinary Portland cement PF42.5, PF32.5 or fly ash Portland cement PF42.5, PF32.5 or composite Portland cement PF42.5, PF32.5.
[0014] As a preferred technical solution of the present invention, the fly ash is any one of Class F and Class C.
[0015] As a preferred technical solution of the present invention, the protective layer in step S4 is any one of ordinary geotextile or plastic film.
[0016] As a preferred technical solution of the present invention, the optimal moisture content in step S2 is determined by a heavy compaction test, and the required amount of water is calculated according to the following formula:
[0017]
[0018] Where m is the required amount of water added, in g, m i is the moisture content ω i The mass of the soil sample at this time is in g, ω i is the original moisture content of the soil sample, in %, ω is the required moisture content, ρ d The dry density is in g / cm 3 , ρ is the wet density g / cm 3 .
[0019] Compared with the prior art, the beneficial effects of the present invention are:
[0020] (1) The present invention recycles and reuses a large amount of industrial steel slag, which reduces environmental pollution and road construction costs, further completing the "dual carbon" construction and generating huge economic benefits. It not only solves economic problems, but also protects the environment by fixing it in the roadbed fill, reduces the pollution problem of steel slag, and has important social and economic effects.
[0021] (2) The present invention proposes to add a large amount of steel slag to the road to improve the clay, thereby increasing the basic mechanical performance parameters of the roadbed fill such as compressive strength, CBR and shear strength, while reducing the damage and destruction of the roadbed fill caused by freeze-thaw cycles, extending the service life of the roadbed, and laying a solid foundation for the construction of long-life roads.
[0022] (3) The present invention determines the appropriate fly ash and cement filling amounts through experiments, and enhances the bonding effect of steel slag and clay through the bonding effect of fly ash and cement, thereby avoiding the problems of looseness, lack of shape, and low strength caused by large amounts of steel slag added to the roadbed fill. In addition, the present invention is targeted at road engineering applications, the raw materials and construction steps are simple, and the applicability is wide. It can be normally used in general projects and has broad application prospects.
[0023] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The invention discloses a large-volume steel slag roadbed filling material and a process flow diagram of the preparation method thereof. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0028] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0029] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0030] Embodiment 1
[0031] Refer to the attached Figure 1As shown, the present invention provides a technical solution: a large-fill steel slag roadbed fill material and a preparation method thereof, comprising stirring and mixing steel slag, cement, fly ash, water and clay to obtain a roadbed fill material, wherein the total mass percentage of the roadbed fill material is 40% of block steel slag, 2% of PC42.5 cement, 6% of F-type fly ash and 58% of clay, wherein the preparation method of the roadbed fill material comprises the following steps:
[0032] S1, crushing steel slag and clay with a jaw crusher, drying them in the sun and air, passing the steel slag through a 20 mm soil sieve, crushing and sieving the sieved part again, selecting the sieve residue with a diameter of less than 20 mm, and storing the collected steel slag and clay under dry and ventilated conditions;
[0033] S2, when preparing in the mixing plant, weigh the dry steel slag, clay, cement, fly ash and water with the corresponding optimal moisture content according to the total mass percentage, first put the steel slag, clay, cement and fly ash less than 20mm into the mixer and stir for 20-40 minutes, then add the water with the optimal moisture content into the mixer and stir for 20-40 minutes, ensure that the mixing is uniform and there is no whitening phenomenon, and cover and transport to the site as soon as possible;
[0034] S3, when mixing on site, weigh dry steel slag, clay, cement, fly ash and water with the corresponding optimum moisture content according to the above total mass percentage, mix the steel slag, clay, cement and fly ash with a size less than 20 mm on site with a mixing machine, mix for 20-40 minutes, add water with a moisture content exceeding 2% of the optimum moisture content, and continue mixing for 20-40 minutes;
[0035] S4, lay the mixed roadbed fill material on the roadbed in a normal layered paving manner, and after rolling and compaction to reach the specified compaction degree, cover the roadbed with a protective layer, complete the natural settlement of the roadbed and the steel slag roadbed fill maintenance for 7 days, and then set up other road structures.
[0036] The embodiment of the present invention is also implemented through the following technical solutions.
[0037] In the embodiment of the present invention, the type of steel slag is massive steel slag after steelmaking.
[0038] In an embodiment of the present invention, the type of cement is any one of ordinary Portland cement PF42.5, PF32.5 or fly ash Portland cement PF42.5, PF32.5 or composite Portland cement PF42.5, PF32.5.
[0039] In the embodiment of the present invention, the fly ash is any one of Class F and Class C.
[0040] In an embodiment of the present invention, the protective layer in step S4 is any one of ordinary geotextile or plastic film.
[0041] In an embodiment of the present invention, the optimum moisture content in step S2 is determined by a heavy compaction test, and the required amount of water is calculated according to the following formula:
[0042]
[0043] Where m is the required amount of water added, in g, m i is the moisture content ω i The mass of the soil sample at this time is in g, ω i is the original moisture content of the soil sample, in %, ω is the required moisture content, and ρd is the dry density, in g / cm 3 , ρ is the wet density g / cm 3 .
[0044] Embodiment 2
[0045] Based on Example 1, the mass proportion of raw materials in the roadbed fill is changed to 45% of block steel slag, 3% of PF42.5 cement, 8% of Class F fly ash and 44% of clay, and the preparation is carried out according to the following steps:
[0046] The preparation method of roadbed fill material comprises the following steps:
[0047] S1, crushing steel slag and clay with a jaw crusher, drying them in the sun and air, passing the steel slag through a 20 mm soil sieve, crushing and sieving the sieved part again, selecting the sieve residue with a diameter of less than 20 mm, and storing the collected steel slag and clay under dry and ventilated conditions;
[0048] S2, when preparing in the mixing plant, weigh the dry steel slag, clay, cement, fly ash and water with the corresponding optimal moisture content according to the total mass percentage, first put the steel slag, clay, cement and fly ash less than 20mm into the mixer and stir for 20-40 minutes, then add the water with the optimal moisture content into the mixer and stir for 20-40 minutes, ensure that the mixing is uniform and there is no whitening phenomenon, and cover and transport to the site as soon as possible;
[0049] S3, when mixing on site, weigh dry steel slag, clay, cement, fly ash and water with the corresponding optimum moisture content according to the above total mass percentage, mix the steel slag, clay, cement and fly ash with a size less than 20 mm on site with a mixing machine, mix for 20-40 minutes, add water with a moisture content exceeding 2% of the optimum moisture content, and continue mixing for 20-40 minutes;
[0050] S4, lay the mixed roadbed fill material on the roadbed in a normal layered paving manner. After rolling and compaction to reach the specified compaction degree, cover the roadbed with a layer of geotextile to complete the natural settlement of the roadbed and the steel slag roadbed fill maintenance for 7 days, and then set up other road structures.
[0051] Embodiment 3
[0052] Based on Example 1, the mass proportion of raw materials in the roadbed fill is changed to 50% block steel slag, 3% PC42.5 cement, 10% Class F fly ash and 37% clay. The steps are consistent with those in Example 1, and a plastic film is selected as the protective layer in step S4.
[0053] Comparative Example 1
[0054] Based on Example 1 to Example 3, the mass proportion of raw materials in the roadbed fill is changed to 20% of block steel slag, 2% of PC42.5 cement and 78% of clay.
[0055] Specifically, the test method tests the maximum dry density, optimum moisture content, liquid limit and plastic limit of the soil improved with large filling amount of steel slag according to the highway geotechnical test regulations, so as to evaluate the road performance and engineering application feasibility of the improved soil. Table 1 is the material ratios of the above-mentioned embodiments and comparative examples, Table 2 is the optimum moisture content determined by compaction test, Table 3 is the liquid limit and plastic limit of the embodiments and comparative examples, and the CBR value is calculated. The unit of CBR is %, p is the unit pressure, the unit is Kpa, and the calculation method is when the penetration is 2.5mm. The load-bearing ratio when the penetration amount is 5 mm is calculated as the verification value. When the CBR when the penetration amount is 5 mm is greater than the CBR when the penetration amount is 2.5 mm, the test should be repeated. The results of the indoor load-bearing ratio test can be used as the basis for the selection of roadbed filling materials and the strength design. The CBR values of the corresponding embodiments and comparative examples are obtained in the test. The test results show that both the embodiments and the comparative examples meet the roadbed requirements of the expressway. It also shows that the recycling of large-fill steel slag and fly ash waste has a good effect.
[0056] Table 1:
[0057]
[0058] Table 2:
[0059]
[0060]
[0061] Table 3:
[0062]
[0063] Table 4:
[0064] Mix ratio Example 1 Example 2 Example 3 Comparative Example 1 CBR / (%) 49.1 59.3 43.8 42.8
[0065] It is worth noting that Chinese patent announcement number CN202311665241.3 A steel slag improved silty clay roadbed material and its filling method and CN115611539B Recycled aggregate, roadbed material and its preparation method prepared by steel slag and phosphogypsum use steel slag with less filling amount.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0067] It should be understood that the specific order or hierarchy of steps in the disclosed process is an example of an exemplary method. Based on design preferences, it should be understood that the specific order or hierarchy of steps in the process can be rearranged without departing from the scope of protection of the present disclosure. The attached method claims present the elements of the various steps in an exemplary order and are not intended to be limited to the specific order or hierarchy described.
[0068] In the above detailed description, various features are grouped together in a single embodiment to simplify the disclosure. This method of disclosure should not be interpreted as reflecting an intention that the embodiments of the claimed subject matter require more features than are clearly stated in each claim. On the contrary, as reflected in the appended claims, the invention is in a state of having less than all the features of the disclosed individual embodiments. Therefore, the appended claims are hereby expressly incorporated into the detailed description, with each claim standing on its own as a separate preferred embodiment of the invention.
[0069] The above description includes examples of one or more embodiments. Of course, it is impossible to describe all possible combinations of components or methods for the purpose of describing the above embodiments, but it should be recognized by those skilled in the art that the various embodiments may be further combined and arranged. Therefore, the embodiments described herein are intended to cover all such changes, modifications and variations that fall within the scope of protection of the appended claims. In addition, with respect to the term "comprising" used in the specification or claims, the word is covered in a manner similar to the term "including", just as "including," is explained as a transitional word in the claims. In addition, any term "or" used in the specification of the claims is intended to mean "non-exclusive or".
Claims
1. A large-volume steel slag roadbed fill material and a preparation method thereof, characterized in that: The method comprises mixing steel slag, cement, fly ash, water and clay to obtain a roadbed fill material, wherein the total mass percentage of the roadbed fill material is 40-65% of steel slag, 1-4% of cement, 5-10% of fly ash, 10-18% of water, and the remainder is clay, wherein the preparation method of the roadbed fill material comprises the following steps: S1, using a jaw crusher to crush steel slag and clay, drying them in the sun and air, passing the steel slag through a 20 mm soil sieve, crushing and sieving the sieved part again, and selecting the sieved part with a diameter less than 20 mm; S2, when preparing in a mixing plant, dry steel slag, clay, cement, fly ash and water with the corresponding optimum moisture content are weighed according to the total mass percentage, firstly steel slag, clay, cement and fly ash with a size less than 20 mm are put into a mixer and stirred for 10-15 minutes, and then water with the optimum moisture content is added into the mixer and stirred for 10-15 minutes; S3, when mixing on site, weigh dry steel slag, clay, cement, fly ash and water with the corresponding optimum moisture content according to the above total mass percentage, mix the steel slag, clay, cement and fly ash with a size less than 20 mm on site with a mixing machine, add water with a moisture content exceeding 2% of the optimum moisture content after mixing for 10-15 minutes, and continue mixing for 10-15 minutes; S4, lay the mixed roadbed fill material on the roadbed in a normal layered paving manner, and after rolling and compaction to reach the specified compaction degree, cover the roadbed with a protective layer, complete the natural settlement of the roadbed and the steel slag roadbed fill maintenance for 7 days, and then set up other road structures.
2. A large-volume steel slag roadbed filling material and a preparation method thereof according to claim 1, characterized in that: The type of the steel slag is massive steel slag after steelmaking.
3. The large-volume steel slag roadbed filling material and the preparation method thereof according to claim 1, characterized in that: The type of cement is any one of ordinary Portland cement PF42.5, PF32.5 or fly ash Portland cement PF42.5, PF32.5 or composite Portland cement PF42.5, PF32.
5.
4. The large-fill steel slag roadbed filling material and the preparation method thereof according to claim 1, characterized in that: The fly ash is any one of Class F and Class C.
5. The large-volume steel slag roadbed filling material and the preparation method thereof according to claim 1, characterized in that: The protective layer in step S4 is any one of ordinary geotextile or plastic film.
6. The large-volume steel slag roadbed filling material and the preparation method thereof according to claim 1, characterized in that: The optimum moisture content in step S2 is determined by a heavy compaction test, and the required amount of water is calculated according to the following formula: Where m is the required amount of water added, in g, m i is the moisture content ω i The mass of the soil sample at this time is in g, ω i is the original moisture content of the soil sample, in %, ω is the required moisture content, ρ d The dry density is in g / cm 3 , ρ is the wet density g / cm 3 .
Citation Information
Patent Citations
Recycled aggregate prepared by steel slag and phosphogypsum, roadbed material and preparation method thereof
CN115611539B
Solid waste-based geocell filler as well as preparation method and application thereof
CN116874271A
Steel slag improved silty clay roadbed material and filling method thereof
CN117661392A
Recycled aggregate composite stabilized soil pavement as well as proportion design method and construction method thereof
CN117888415A
Production method of subbase material for road
JP2019172557A