Europium-barium-copper oxide waste target recycling method
Through physical crushing and pressure grouting molding technology, the waste target of europium barium copper oxide is directly recovered, solving the problem of large and complex energy consumption of rare earth metal recycling in the existing technology, and achieving high efficiency of high-density europium barium copper oxide targets Preparation, simplifying the process flow and reducing contamination.
Patent Information
- Application Number
- CN202410955887.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing superconducting target recycling methods, the recycling process of rare rare earth metals consumes a lot of energy, is complex and not environmentally friendly, especially the use of hydrogen reduction method for equipment and safety requirements, and the wet and pyrometallurgical processes require complex oxides. The powder preparation process increases production costs.
The waste target of europium barium copper oxide was directly crushed by physical method, and nano-scale particles were obtained after three pulverization, and slurry with a solid content of 50-75%. The high-density target material blank was obtained through pressure grouting molding technology, which was dried and Degreasing and sintering treatments to prepare high-performance europium barium copper oxide targets, omitting chemical reactions and complex powder preparation processes.
It realizes efficient recycling and reuse of europium barium copper oxide targets, simplifies the process flow, reduces energy consumption and pollution, improves production efficiency and product density, reaches 95%, and is environmentally friendly and pollution-free.
Smart Images

Figure CN118908713A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of superconducting target materials, and in particular relates to a method for recycling waste europium barium copper oxide targets. Background Art
[0002] At present, the most studied superconducting target materials and thin films are the yttrium barium copper oxide series, that is, other trace elements are added to YCBO. Most of these added elements are lanthanide elements, such as praseodymium (Pr), curium (Pm), samarium (Sm), dysprosium (Dy), holmium (Ho), etc., to form superconducting films such as Y1-xHoxBa2Cu3O7-δ. The reason for this is that rare earth elements have different outer electron structures and ionic radii from yttrium. When they partially or even completely replace yttrium, they may cause changes on the atomic scale and changes in the electronic structure of oxide superconductors to improve their performance indicators.
[0003] The latest research shows that EBCO films have leading advantages in increasing the critical superconducting temperature (Tc) and critical current density (Jc) and improving the corresponding sensitivity to magnetic fields or frequency width. Therefore, the preparation of qualified EBCO targets is of great significance in the study of superconducting mechanisms and properties of superconducting materials, as well as the development of practical devices.
[0004] At present, the recovery of rare earth metals from oxide waste targets is mainly divided into wet and pyrometallurgical recovery, such as acid dissolution, reduction, vacuum distillation, extraction, etc. These methods mainly involve acid dissolution, replacement, electrolysis and other steps, and have high energy consumption. When using the reduction method, hydrogen is generally used as a reducing agent, which has high requirements for equipment and safety protection measures and is not conducive to low-carbon environmental protection. After using wet and pyrometallurgical processes to recover precious rare earth metals, the rare earth metals need to be prepared into oxide powders and then prepared into targets. The overall process is complicated and increases production costs. Summary of the invention
[0005] In view of this, some embodiments disclose a method for recycling waste europium barium copper oxide targets to finally obtain europium barium copper oxide, the method comprising the steps of:
[0006] S1. Pre-treating the waste target of europium barium copper oxide;
[0007] S2, crushing the pretreated europium barium copper oxide waste target three times to obtain nano-scale particles; wherein:
[0008] After the first crushing, the blocky waste target of europium barium copper oxide is crushed into millimeter-sized particles of europium barium copper oxide;
[0009] After the second crushing, the millimeter-sized particles of europium barium copper oxide are crushed into micrometer-sized particles of europium barium copper oxide;
[0010] After the third pulverization, the europium barium copper oxide micron-sized particles are prepared into a slurry, and the slurry is sand-milled to obtain europium barium copper oxide nano-sized particles;
[0011] S3, mixing the europium barium copper oxide nanoparticles with water, a dispersant, and a binder in a set proportion to obtain a europium barium copper oxide slurry; wherein the mass content of the europium barium copper oxide is 50-75%;
[0012] S4, obtaining a europium barium copper oxide target blank by pressure injection of europium barium copper oxide slurry;
[0013] S5. The europium barium copper oxide target blank is dried, degreased and sintered to obtain a europium barium copper oxide target.
[0014] Furthermore, in some embodiments of the method for recycling and reusing waste europium barium copper oxide targets, in step S1, the pretreatment of the waste europium barium copper oxide targets includes surface cleaning and preliminary crushing, the surface of the waste europium barium copper oxide targets is wiped clean with sandpaper and alcohol, and the waste targets are preliminarily crushed into blocks with a size less than 5 cm using a blunt-tipped instrument.
[0015] Some embodiments disclose a method for recycling and reusing waste europium barium copper oxide targets. In step S2, during the first crushing, a jaw crusher is used to crush the blocky europium barium copper oxide waste targets into millimeter-sized particles of europium barium copper oxide, and the particle size of small particles is less than 5 mm; during the second crushing, an ultrafine air flow mill is used to crush the millimeter-sized particles of europium barium copper oxide into micron-sized particles of europium barium copper oxide, and the particle size D50 is 2 to 5 μm; during the third crushing, a sand mill is used to sand grind the slurry to obtain europium barium copper oxide nanoparticles with an average particle size of 200 to 800 nm.
[0016] In some embodiments of the present invention, the method for recycling waste europium barium copper oxide targets disclosed in step S4 includes:
[0017] The europium barium copper oxide slurry is injected into a pressure mold for molding, the injection time is 3 to 6 hours, the injection pressure is 0.01 to 0.5 Pa, and a molded green blank is obtained.
[0018] In the method for recycling waste europium barium copper oxide targets disclosed in some embodiments, in step S5, the drying process of the formed green blank comprises:
[0019] The formed green body is first dried for 24 to 36 hours at a first drying temperature of 25 to 35° C. and a first relative humidity of 70% to 80%;
[0020] Then, the formed green blank is dried for a second time for 36 to 48 hours at a second drying temperature of 35 to 45° C. and a second relative humidity of 70 to 80% to obtain a target material green blank having a relative density greater than 65%.
[0021] Some embodiments disclose a method for recycling and reusing waste europium barium copper oxide targets. In step S5, the degreasing temperature of the target blank is set to 500-800°C, the degreasing heating rate is set to 0.5-1.5°C / min, and the degreasing holding time is set to 6-30h.
[0022] In the method for recycling waste europium barium copper oxide targets disclosed in some embodiments, the degreasing process in step S5 includes:
[0023] Heating from room temperature to the first step temperature of 300°C at a heating rate of 0.5°C / min, and keeping the temperature for 1 to 10 hours;
[0024] The temperature was raised from the first step temperature to the second step temperature of 650°C at a heating rate of 0.5°C / min, and kept at this temperature for 5 to 20 hours;
[0025] The temperature was lowered from the second step temperature to the third step temperature of 500°C at a cooling rate of 1°C / min, and then cooled naturally.
[0026] In the method for recycling and reusing waste europium barium copper oxide targets disclosed in some embodiments, the temperature of the sintering treatment in step S5 is 900-950° C., and the sintering time is 0.5-20 hours.
[0027] In the method for recycling waste europium barium copper oxide targets disclosed in some embodiments, the sintering process in step S5 includes:
[0028] Heating from room temperature to 900-950°C at a rate of 1-2°C / min, and keeping at this temperature for 0.5-20h;
[0029] The temperature was lowered to 500°C at a cooling rate of 3°C / min, and then cooled naturally.
[0030] In the method for recycling and reusing waste europium barium copper oxide targets disclosed in some embodiments, in step S5, the degreasing and sintering processes are carried out in an atmosphere of air, oxygen or nitrogen.
[0031] The method for recycling and reusing waste europium barium copper oxide targets disclosed in the embodiment of the present invention directly crushes the waste europium barium copper oxide targets by physical methods, obtains nanometer-level waste europium barium copper oxide target nanopowder after three crushing processes, and then prepares the europium barium copper oxide nanopowder into a slurry with a solid content of 50-75%, and adopts pressure grouting molding technology to obtain a high-density target blank, and prepares a high-performance europium barium copper oxide target material after degreasing and sintering, with an average grain size of 20 μm and a density of 95%. The process of the method disclosed in the embodiment of the present invention does not involve complex chemical reactions, and only uses physical methods to recycle waste europium barium copper oxide targets, omitting the complex process of re-preparing oxidized powder after traditional wet recovery and pyrometallurgical recovery of metal europium, making the recycling and preparation process simpler, and environmentally friendly and pollution-free, and is a practical method for recycling and reusing waste europium barium copper oxide targets to prepare europium barium copper oxide targets. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A flow chart of a method for recycling and reusing waste europium barium copper oxide targets disclosed in some embodiments. DETAILED DESCRIPTION
[0033] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.
[0034] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.
[0035] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0036] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0037] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.
[0038] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.
[0039] In some embodiments, Figure 1 As shown, the method for recycling waste europium barium copper oxide targets comprises the following steps:
[0040] S1. Pre-treating the waste target of europium barium copper oxide; generally, the chemical composition and purity of the waste target raw material of europium barium copper oxide (EBCO) are not changed after magnetron sputtering, and the impurity content is extremely low, so the purity of the waste target powder can meet the requirements for preparing europium barium copper oxide target material, so after pre-treating the waste target of europium barium copper oxide, it is used as a raw material for subsequent processes to finally prepare europium barium copper oxide target material;
[0041] S2, crushing the pretreated europium barium copper oxide waste target three times to obtain nano-scale particles; wherein:
[0042] After the first crushing, the blocky waste target of europium barium copper oxide is crushed into millimeter-sized particles of europium barium copper oxide;
[0043] After the second crushing, the millimeter-sized particles of europium barium copper oxide are crushed into micrometer-sized particles of europium barium copper oxide;
[0044] After the third crushing, the europium barium copper oxide micron-sized particles are prepared into a slurry, and the slurry is sand-milled to obtain europium barium copper oxide nano-sized particles; usually, the europium barium copper oxide micron-sized particles need to be mixed with a certain mass of water and a dispersant to obtain a slurry with a certain solid content, and then the slurry is sand-milled; usually, the mass content of the europium barium copper oxide micron-sized particles in the slurry is 50-75%, the content of the dispersant is 1-2%, and the balance is deionized water; wherein the dispersant is a polyacrylic acid dispersant;
[0045] S3, mixing europium barium copper oxide nanoparticles with water, a dispersant, and a binder in a set ratio to obtain europium barium copper oxide slurry; wherein the mass content of europium barium copper oxide is 50-75%, the content of the dispersant is 1-2%, the content of the binder is 1-2%, and the balance is deionized water; wherein the dispersant is a polyacrylic acid dispersant, and the binder is a vinyl alcohol binder;
[0046] S4, europium barium copper oxide slurry is subjected to pressure grouting to obtain europium barium copper oxide target blank; in some embodiments, the europium barium copper oxide slurry is injected into a pressure mold for molding, the grouting time is 3 to 6 hours, the grouting pressure is 0.01 to 0.5 Pa, and a molded blank is obtained; usually, the europium barium copper oxide target is prepared into a europium barium copper oxide target blank in a mold using a new pressure grouting molding process, and the relative density of the target blank is greater than 65%; usually, the mold is made of high-strength water-absorbing gypsum powder;
[0047] As an optional embodiment, the europium barium copper oxide slurry is subjected to vacuum defoaming treatment before pressure grouting molding, and the vacuum pressure is less than 0.1 Pa;
[0048] S5. The europium barium copper oxide target blank is dried, degreased and sintered to obtain a europium barium copper oxide target. Usually, the europium barium copper oxide target blank is dried at a constant temperature and humidity; as an optional implementation, the constant temperature and humidity drying process can be carried out in a constant temperature and humidity chamber in two stages, and finally a target blank with a constant weight is obtained; usually, the degreasing and sintering process of the europium barium copper oxide target blank is carried out in an air, oxygen or nitrogen atmosphere.
[0049] As a more preferred embodiment, the degreasing and sintering process of the europium barium copper oxide target blank is carried out in a flowing air, oxygen or nitrogen gas flow, and the gas flow rate is set to 5-15 L / min.
[0050] In some embodiments, the pretreatment of the waste europium barium copper oxide target includes surface cleaning and preliminary crushing. The surface of the waste europium barium copper oxide target is wiped clean with sandpaper and alcohol, and the waste target is crushed into blocks with a size less than 5 cm using a blunt-tip instrument.
[0051] In some embodiments, the step of crushing the waste target of europium barium copper oxide specifically includes:
[0052] During the first crushing, a jaw crusher is used to crush the blocky waste target of europium barium copper oxide into millimeter-sized particles of europium barium copper oxide, and small particles with a particle size of less than 5 mm are recovered;
[0053] During the second crushing, the millimeter-sized particles of europium barium copper oxide are crushed into micrometer-sized particles of europium barium copper oxide by using an ultrafine airflow mill, and the particle size D50 is 2 to 5 μm; usually, the particle size can be measured by a laser particle size analyzer to obtain the D50 value;
[0054] During the third pulverization, the slurry is sand-milled using a sand mill to obtain europium barium copper oxide nanoparticles with an average particle size of 200 to 800 nm, which can be measured using a laser force analyzer. Usually, the slurry is sand-milled in a sand mill, and then the sand-milled slurry is placed in a drying oven at 70 to 90° C. and dried for 24 to 48 hours to obtain europium barium copper oxide nanoparticles.
[0055] In some embodiments, the drying process of the formed green billet in step S5 includes:
[0056] The formed green blank is first dried for 24 to 36 hours at a first drying temperature of 25 to 35° C. and a first relative humidity of 70% to 80%;
[0057] Then, the formed green blank is dried for a second time for 36 to 48 hours at a second drying temperature of 35 to 45° C. and a second relative humidity of 70 to 80% to obtain a target material green blank having a relative density greater than 65%.
[0058] In some embodiments, in step S5, the degreasing temperature of the target blank is set to 500-800°C, the degreasing heating rate is set to 0.5-1.5°C / min, and the degreasing holding time is set to 6-30h.
[0059] In some embodiments, the degreasing process in step S5 includes:
[0060] Heating from room temperature to the first step temperature of 300°C at a heating rate of 0.5°C / min, and keeping the temperature for 1 to 10 hours;
[0061] The temperature was raised from the first step temperature to the second step temperature of 650°C at a heating rate of 0.5°C / min, and kept at this temperature for 5 to 20 hours;
[0062] The temperature was lowered from the second step temperature to the third step temperature of 500°C at a cooling rate of 1°C / min, and then cooled naturally.
[0063] In some embodiments, the sintering temperature in step S5 is 900-950° C., and the sintering time is 0.5-20 h.
[0064] In some embodiments, the sintering process in step S5 includes:
[0065] Heating from room temperature to 900-950°C at a rate of 1-2°C / min, and keeping at this temperature for 0.5-20h;
[0066] The temperature was lowered to 500°C at a cooling rate of 3°C / min, and then cooled naturally.
[0067] The technical details are further illustrated below in conjunction with embodiments.
[0068] Example 1
[0069] In Example 1, the method for recycling waste europium barium copper oxide targets comprises the following steps:
[0070] (1) Clean the surface of the EBCO waste target with sandpaper and alcohol, and use a hammer to initially break the waste target into pieces less than 2 cm in size to obtain the pretreated EBCO waste target.
[0071] (2) The pretreated EBCO waste target is crushed three times. The first step is to crush the blocky EBCO waste target into particles of about 3 mm using a jaw crusher; the second step is to further crush the 3 mm particles into particles with an average particle size of 3 μm using an ultrafine air flow mill; the third step is to use a sand mill to prepare a slurry made of micron powder, wherein the solid content of the slurry is 70% and the dispersant is 1% of a polyurethane dispersant; further refine and crush it into EBCO particles with a D50 of 300 nm; the sand-milled slurry is placed in a drying oven at 80° C. and dried for 48 hours before being ground into nano powder.
[0072] (3) The nano powder obtained by the third step of crushing is mixed with water, polyacrylamide and polyurethane in a set proportion to obtain an EBCO slurry with a solid content of 60%, wherein the mass content of EBCO is 60%, the mass content of polyacrylamide is 1%, the mass content of polyurethane is 1%, and the balance is deionized water.
[0073] (4) An EBCO blank with a density of 63% was obtained by pressure grouting, wherein the grouting pressure was 0.15 MPa and the grouting time was 2 h.
[0074] (5) The EBCO target blank is dried at a constant temperature and humidity; the first drying is performed at a first drying temperature of 35° C. and a first humidity of 80% RH for 36 hours; and the second drying is performed at a second drying temperature of 45° C. and a second humidity of 80% RH for 48 hours.
[0075] (6) The dried EBCO target blank was degreased, and the specific parameters were as follows: the temperature was set at 600°C, the degreasing heating rate was 0.5°C / min, and the degreasing holding time was 20h; then it was sintered, and the sintering temperature was set as follows: heating from room temperature to 920°C at 2°C / min, holding for 20h; cooling to 500°C at 3°C / min, and cooling naturally.
[0076] The average grain size of the EBCO target was measured by SEM, and the average grain size was 18.2 μm. The relative density of EBCO was measured by Archimedes drainage method, and the relative density was 95.8%.
[0077] Example 2
[0078] In Example 2, the method for recycling waste europium barium copper oxide targets comprises the following steps:
[0079] (1) Wipe and clean the surface of the EBCO waste target with sandpaper and alcohol, and use an impact press to initially break the waste target into blocks less than 5 cm in size to obtain a pretreated EBCO waste target.
[0080] (2) The pretreated EBCO waste target is crushed three times. The first step is to crush the blocky EBCO waste target into 5 mm particles using a jaw crusher; the second step is to further crush the EBCO waste target particles into particles with an average particle size of 5 μm using an ultrafine air flow mill; the third step is to use a sand mill to further refine and crush the slurry prepared from the powder in the second step, wherein the solid content of the slurry is 70% and the dispersant is 1% of a polyurethane dispersant; into EBCO particles with a D50 of 500 nm; the sand-milled slurry is placed in a drying oven at 80° C. and dried for 36 hours before being ground into nano powder.
[0081] (3) The nano powder obtained by the third step of crushing is mixed with water, methyl amyl alcohol and polyvinyl acetate in a set proportion to obtain an EBCO slurry with a solid content of 75%, wherein the mass content of EBCO is 75%, the mass content of methyl amyl alcohol is 1%, the mass content of polyvinyl acetate is 1%, and the balance is deionized water.
[0082] (4) An EBCO blank with a density of 65% was obtained by pressure grouting, wherein the grouting pressure was 0.1 MPa and the grouting time was 3 h.
[0083] (5) The EBCO target blank is dried at a constant temperature and humidity; the first drying is performed at a first drying temperature of 35° C. and a first humidity of 80% RH for 36 hours; and the second drying is performed at a second drying temperature of 45° C. and a second humidity of 80% RH for 48 hours.
[0084] (6) The dried EBCO target blank was degreased, and the specific parameters were as follows: the temperature was set to 500°C, the degreasing heating rate was 1°C / min, and the degreasing holding time was 24h; then it was sintered, and the sintering temperature was set to: increase the temperature from room temperature to 950°C at 2°C / min, hold for 18h, cool down to 500°C at 3°C, and cool naturally.
[0085] The average grain size of the EBCO target was measured by SEM, and the average grain size was 19.8 μm. The relative density of EBCO was measured by Archimedes drainage method, and the relative density was 95.2%.
[0086] Example 3
[0087] In Example 3, the method for recycling waste europium barium copper oxide targets comprises the following steps:
[0088] (1) Wipe and clean the surface of the EBCO waste target with sandpaper and alcohol, and use a hammer to initially break the waste target into blocks less than 5 cm in size to obtain the pretreated EBCO waste target.
[0089] (2) The pretreated EBCO waste target is crushed three times. The first step is to crush the blocky EBCO waste target into 2 mm particles using a jaw crusher; the second step is to further crush the EBCO waste target particles into particles with an average particle size of 4 μm using an ultrafine air flow mill; the third step is to use a sand mill to further refine and crush the slurry prepared from the powder in the second step, wherein the solid content of the slurry is 70% and the dispersant is 1% of a polyurethane dispersant; into EBCO particles with a D50 of 400 nm; the sand-milled slurry is placed in a drying oven at 80° C. and dried for 48 hours before being ground into nano powder.
[0090] (3) The nano powder obtained in the third step of pulverization is mixed with water, gum and cellulose nitrate in a set ratio to obtain an EBCO slurry with a solid content of 55%, wherein the mass content of EBCO is 55%, the mass content of gum is 1%, the mass content of cellulose nitrate is 1%, and the balance is deionized water.
[0091] (4) An EBCO blank with a density of 60% is obtained by pressure grouting, wherein the grouting pressure is 0.25 MPa and the grouting time is 2 h.
[0092] (5) The EBCO target blank is dried at a constant temperature and humidity; the first drying is performed at a first drying temperature of 35° C. and a first humidity of 80% RH for 36 hours; and the second drying is performed at a second drying temperature of 45° C. and a second humidity of 80% RH for 48 hours.
[0093] (6) The dried EBCO target blank was degreased, and the specific parameters were as follows: the temperature was set at 700°C, the degreasing heating rate was 0.8°C / min, and the degreasing holding time was 20h. Then, the sintering treatment was carried out, and the sintering temperature was set as follows: heating from room temperature to 900°C at 1°C / min, holding for 20h, cooling to 500°C at 3°C / min, and cooling naturally.
[0094] The average grain size of the EBCO target was measured by SEM, and the average grain size was 18.2 μm. The relative density of EBCO was measured by Archimedes drainage method, and the relative density was 95.0%.
[0095] The method for recycling and reusing waste europium barium copper oxide targets disclosed in the embodiment of the present invention directly crushes the waste europium barium copper oxide targets by physical methods, obtains nanometer-level waste europium barium copper oxide target nanopowder after three crushing processes, and then prepares the europium barium copper oxide nanopowder into a slurry with a solid content of 50-75%, and adopts pressure grouting molding technology to obtain a high-density target blank, and prepares a high-performance europium barium copper oxide target material after degreasing and sintering, with an average grain size of 20 μm and a density of 95%. The process of the method disclosed in the embodiment of the present invention does not involve complex chemical reactions, and only uses physical methods to recycle waste europium barium copper oxide targets, omitting the complex process of re-preparing oxidized powder after traditional wet recovery and pyrometallurgical recovery of metal europium, making the recycling and preparation process simpler, and environmentally friendly and pollution-free, and is a practical method for recycling and reusing waste europium barium copper oxide targets to prepare europium barium copper oxide targets.
[0096] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. Method for recycling waste targets of europium barium copper oxide, It is characterized in that The method comprises the steps of: S1. Pre-treating the waste target of europium barium copper oxide; S2, crushing the pretreated europium barium copper oxide waste target three times to obtain nano-scale particles; wherein: After the first crushing, the blocky waste target of europium barium copper oxide is crushed into millimeter-sized particles of europium barium copper oxide; After the second crushing, the millimeter-sized particles of europium barium copper oxide are crushed into micrometer-sized particles of europium barium copper oxide; After the third pulverization, the europium barium copper oxide micron-sized particles are prepared into a slurry, and the slurry is sand-milled to obtain europium barium copper oxide nano-sized particles; S3, mixing the europium barium copper oxide nanoparticles with water, a dispersant, and a binder in a set proportion to obtain a europium barium copper oxide slurry; wherein the mass content of the europium barium copper oxide is 50-75%; S4, obtaining a europium barium copper oxide target blank by pressure injection of europium barium copper oxide slurry; S5. The europium barium copper oxide target blank is dried, degreased and sintered to obtain a europium barium copper oxide target.
2. The method for recycling waste europium barium copper oxide targets according to claim 1, It is characterized in that In step S1, the pretreatment of the waste target of europium barium copper oxide includes surface cleaning and preliminary crushing. The surface of the waste target of europium barium copper oxide is wiped clean with sandpaper and alcohol, and the waste target is preliminarily crushed into blocks with a size less than 5 cm using a blunt-tip instrument.
3. The method for recycling waste europium barium copper oxide targets according to claim 1, It is characterized in that In step S2: During the first crushing, a jaw crusher is used to crush the blocky waste target of europium barium copper oxide into millimeter-sized particles of europium barium copper oxide, and the particle size of small particles is less than 5mm; During the second pulverization, the millimeter-sized particles of europium barium copper oxide are pulverized into micrometer-sized particles of europium barium copper oxide by ultrafine jet milling, and the particle size D50 is 2 to 5 μm; During the third pulverization, the slurry is sand-milled by a sand mill to obtain europium barium copper oxide nanoparticles with an average particle size of 200 to 800 nm.
4. The method for recycling waste europium barium copper oxide targets according to claim 1, It is characterized in that In step S4, the method for obtaining a europium barium copper oxide target blank by pressure grouting comprises: The europium barium copper oxide slurry is injected into a pressure mold for molding, the injection time is 3 to 6 hours, the injection pressure is 0.01 to 0.5 Pa, and a molded green blank is obtained.
5. The method for recycling waste europium barium copper oxide targets according to claim 1, It is characterized in that In step S5, the drying process of the formed green billet includes: The formed green body is first dried for 24 to 36 hours at a first drying temperature of 25 to 35° C. and a first relative humidity of 70% to 80%; Then, the formed green blank is dried for a second time for 36 to 48 hours at a second drying temperature of 35 to 45° C. and a second relative humidity of 70 to 80% to obtain a target material green blank having a relative density greater than 65%.
6. The method for recycling waste europium barium copper oxide targets according to claim 1, It is characterized in that In step S5, the degreasing temperature of the target blank is set to 500-800°C, the degreasing heating rate is set to 0.5-1.5°C / min, and the degreasing holding time is set to 6-30h.
7. The method for recycling waste europium barium copper oxide targets according to claim 6, It is characterized in that The degreasing process in step S5 includes: Heating from room temperature to the first step temperature of 300°C at a heating rate of 0.5°C / min, and keeping the temperature for 1 to 10 hours; The temperature was raised from the first step temperature to the second step temperature of 650°C at a heating rate of 0.5°C / min, and kept at this temperature for 5 to 20 hours; The temperature was lowered from the second step temperature to the third step temperature of 500°C at a cooling rate of 1°C / min, and then cooled naturally.
8. The method for recycling waste europium barium copper oxide targets according to claim 1, It is characterized in that The sintering temperature in step S5 is 900-950° C., and the sintering time is 0.5-20 hours.
9. The method for recycling waste europium barium copper oxide targets according to claim 8, It is characterized in that The sintering process in step S5 includes: Heating from room temperature to 900-950°C at a rate of 1-2°C / min, and keeping at this temperature for 0.5-20h; The temperature was lowered to 500°C at a cooling rate of 3°C / min, and then cooled naturally.
10. The method for recycling waste europium barium copper oxide targets according to claim 1, It is characterized in that In step S5, the debinding and sintering process is performed in an air, oxygen or nitrogen atmosphere.
Citation Information
Patent Citations
Preparation method of nanometer pearl powder
CN101695504A
Lanthanum zironate based ceramic target material for electron beam physical vapor deposition and preparation method thereof
CN107903060A
Preparation method for producing ITO target material by directly crushing and pulverizing ITO waste target
CN112079627A
Preparation method of europium-barium-copper oxide superconducting sputtering target material and product of europium-barium-copper oxide superconducting sputtering target material
CN116606131A
A manufacturing method of ITO powder collected from a waste ITO sputtering target for producing high density target and a manufacturing method of sputtering target
KR100637868B1
Cited By
Preparation method of nanoscale high-purity superconducting powder
CN122531881A