Refractory brick for steel furnace lining and preparation method thereof
By using specific combination materials and bonding agents in refractory bricks to form MgAlON structures, the problems of short life and poor erosion resistance in low-sulfur steel smelting are solved, and higher refractory performance and a wider range of application are achieved. It reduces production costs and is in line with the concept of green and sustainable development.
Patent Information
- Application Number
- CN202411009512.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-26
AI Technical Summary
In the existing low-sulfur steel smelting, the refractory bricks have short service life and poor anti-erosion and peeling effects, resulting in increased maintenance costs and safety hazards. The addition of a large number of CaO and CaF2 causes serious erosion to the furnace-lined refractory bricks.
Using large crystalline electromelted magnesium sand, coarse dicalcium electromelted magnesium sand, electromelted spinel, sintered spinel, bimodal alumina, AlSi12 alloy, Al-Mg alloy and boron carbide and other materials, combined with phenolic resin or magnesium As a binding agent, aluminum gel is formed by high-pressure molding and high-temperature sintering to form refractory bricks with MgAlON structure, improving corrosion resistance and high-temperature performance.
It extends the service life of refractory bricks, improves the resistance to erosion and peeling resistance, reduces maintenance costs, adapts to different smelting conditions, meets the requirements of green and sustainable development, and improves the production efficiency and quality of steel smelting.
Smart Images

Figure CN118908739A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of refractory bricks, in particular to a refractory brick for steelmaking furnace lining and a preparation method thereof. Background Art
[0002] The sulfur content in steel products will directly affect the corrosion resistance, fatigue characteristics, welding performance, toughness and plasticity of the structure. Therefore, it is necessary to control the sulfur content in the raw materials of steel products and remove it by using RH, LF, KR and other liquid steel refining and desulfurization technologies. The common desulfurization process is to use lime powder as a desulfurizer, which can contact with the sulfur diffused to the surface, react chemically, and diffuse the desulfurized products at the reaction interface. Desulfurization reaction equation: S+O 2- =S 2- +O.
[0003] Alkaline oxides can provide oxygen ions to the slag, so appropriately increasing the slag alkalinity can promote the desulfurization reaction process; and the desulfurization reaction is an endothermic reaction at the slag-gold interface. To improve the desulfurization effect, it is necessary to increase the mass transfer coefficient and increase the reaction interface area. Therefore, strengthening stirring and increasing the reaction temperature are necessary parts of the desulfurization process.
[0004] The smelting process of high-quality low-sulfur steel is mostly based on the CaO-CaF2 slag system, adding appropriate amounts of Al2O3, MgO, and SiO2, and adjusting the CaF2 component ratio according to the sulfur content requirements of different steel grades. However, the addition of a large amount of CaO and CaF2 causes serious erosion of the furnace lining refractory bricks, and the ultra-high smelting temperature has higher performance requirements for the furnace lining materials. In addition, the refractory bricks currently used for low-sulfur steel smelting generally have problems such as short service life, poor corrosion resistance, and poor spalling resistance, which leads to increased maintenance costs and safety hazards. Summary of the invention
[0005] In order to solve the deficiencies in the prior art, the present invention provides a refractory brick for a steelmaking furnace lining and a preparation method thereof. The refractory brick can be used in the desulfurization smelting of steel grades, is suitable for different desulfurization requirements and different smelting conditions, and has the advantages of long service life, good corrosion resistance and anti-stripping effect.
[0006] In order to achieve the above object, the specific scheme adopted by the present invention is: In one aspect, the present invention provides a refractory brick for a steelmaking furnace lining, wherein the components and their mass percentages are as follows: Large crystal fused magnesia 35-40%; Coarse dicalcium fused magnesia 20-25%; Fine dicalcium fused magnesia 15-20%; Fused spinel 4-8%; Sintered spinel 4-8%; Bimodal alumina 4-8%; AlSi12 alloy 5-10%; Al-Mg alloy 2-5%; Boron carbide 2-5%; The sum of the mass percentages of each component is 100%.
[0007] Furthermore, a binder accounting for 3-7% of the total mass of the refractory brick is added to the refractory brick, and the binder is any one of the following: (a) phenolic resin; (ii) phenolic resin and magnesium aluminum gel are mixed in a mass percentage of 1:0.43; (3) Mixing magnesium aluminum gel dry powder and deionized water in a mass percentage of 1:0.3; The viscosity of the phenolic resin used in (i) and (ii) is 22000-24000 MPa﹒ s, and the residual carbon content is 6%; the magnesium aluminum gel used in (ii) is prepared by mixing magnesium aluminum gel dry powder and water in a mass ratio of 1:0.18, and the particle size of the magnesium aluminum gel dry powder is less than 100 nm.
[0008] Further, the particle size of the large crystal fused magnesia is 4 to 1 mm; The particle size of coarse dicalcium fused magnesia is 1-0mm; The particle size of fine dicalcium fused magnesia is 200 mesh; Fused spinel 5μm; Sintered spinel 2-5μm; Bimodal alumina 5μm; AlSi12 alloy 10μm; Al-Mg alloy 100 μm; Boron carbide 350 mesh.
[0009] Furthermore, the content of periclase in the large crystal fused magnesia is >97%; In dicalcium fused magnesia, the content of MgO is 96-99%, and the ratio of impurity phase CaO to SiO2 is 2; In fused spinel, the MgO content is >78%; Bimodal alumina is an activated alumina powder with a bimodal distribution of particle size; In sintered spinel, the Al2O3 content is greater than 76%; In Al-Mg alloy, the Al content is greater than 47%.
[0010] On the other hand, the present invention provides a method for preparing refractory bricks for steelmaking furnace lining, which mainly comprises the following steps: Step 1, placing large crystalline fused magnesia, coarse dicalcium fused magnesia, fused spinel, sintered spinel, bimodal alumina, AlSi12 alloy and Al-Mg alloy in a blender according to mass percentage and stirring evenly to obtain a granular mixture; Place fine dicalcium fused magnesia sand and boron carbide in a mixer and stir evenly to obtain a fine powder mixture; Step 2: Add a binder to the granular mixture and mix them evenly, then add the fine powder mixture and mix them evenly to obtain a mud material; Step 3, treating the mud material; Step 4: placing the clay material in a mixer, stirring and mixing to obtain a mixed material; Step 5: High pressure forming the mixed material under a pressure of 630T to 2500T to obtain a brick; Step 6: Baking the bricks to obtain refractory bricks.
[0011] Furthermore, in step three, the material trapping time is 3-4 days.
[0012] Furthermore, in step 4, during the stirring and mixing process, 0-5% of a binder is added according to the binding conditions of the clay materials, and the total amount of the binder added in step 2 and step 4 accounts for 3-7% of the total mass of the refractory bricks.
[0013] Furthermore, the binder is any one of the following: (a) phenolic resin; (ii) phenolic resin and magnesium aluminum gel are mixed in a mass percentage of 1:0.43; (3) Mixing magnesium aluminum gel dry powder and deionized water in a mass percentage of 1:0.3; The viscosity of the phenolic resin used in (i) and (ii) is 22000-24000 MPa﹒s, and the residual carbon content is 6%; The magnesium aluminum gel used in (ii) is prepared by mixing magnesium aluminum gel dry powder and water in a mass ratio of 1:0.18, and the particle size of the magnesium aluminum gel dry powder is less than 100 nm.
[0014] Furthermore, different binders are added and the baking parameters are also different, among which: Case 1: When the binder is phenolic resin, the baking parameters are: 80-100℃ for 8 hours in air atmosphere and 190-200℃ for 16 hours; Case 2: When the binder is a mixture of phenolic resin and magnesium aluminum gel, the baking parameters are: 330-350℃ for 16 hours in air atmosphere; Case 3: When the binder is a mixture of magnesium aluminum gel dry powder and deionized water, the baking parameters are: 100-110°C for 24 hours in an air atmosphere.
[0015] Furthermore, the refractory bricks obtained in step six are subjected to high-temperature sintering in a nitrogen atmosphere, the sintering temperature of the high-temperature sintering operation is 1600-1750° C., and the insulation time is 1-3 hours.
[0016] Among them, large-crystal fused magnesia, coarse dicalcium fused magnesia and fine dicalcium fused magnesia are used as aggregates, fused spinel, sintered spinel and bimodal alumina are used as matrices, and AlSi12 alloy, Al-Mg alloy and boron carbide are used as reaction precursors.
[0017] The present invention selects large-crystal fused magnesia with a periclase content greater than 97% and a good crystal development degree, and coarse dicalcium fused magnesia with a MgO content of 96-99% and a ratio of impurity phase CaO to SiO2 of approximately 2 as aggregate. Due to the excellent high-temperature resistance of periclase, the selection of large-crystal fused magnesia with a good crystallization degree can directly improve the high-temperature performance of the product. In the impurity components of the crude dicalcium fused magnesia selected by the present invention, when the calcium-silicon ratio is less than 1.87, the periclase bonding phase is low-melting-point calcium-forsterite or magnesium rhodonite, and when it is greater than 1.87, the bonding phase is high-melting-point dicalcium silicate or tricalcium silicate, and the impurity content of the product is strictly controlled, which is helpful to improve various performances of the product; free calcium oxide and silicon dioxide exist in the form of liquid phase at high temperature due to their low melting points, and can diffuse into the inside of the blank matrix, forming transcrystalline cracks inside the periclase, which are diffused and filled by the binder, greatly improving the high-temperature mechanical properties of the product; the crude dicalcium fused magnesia with a calcium-silicon ratio close to 2 is selected, and the high-temperature performance of the product can be further improved on the basis of ensuring the development degree of periclase.
[0018] When selecting the matrix raw material, the present invention selects fine dicalcium fused magnesia, fused spinel, sintered spinel and bimodal alumina for compounding, and adds them in the form of ultrafine powder. The compounded raw material components contain a periclase phase or a corundum phase with high activity, which can produce an in-situ spinelization reaction at high temperature, promote high-temperature sintering of the product, and improve the product strength. Among them, the reason for selecting bimodal alumina is that the laser particle size distribution curve of bimodal alumina has two peaks, compared with the single-peak alumina with only one peak in the particle size distribution curve and relatively concentrated particle size, the particle size distribution range of bimodal alumina is wider and more uniform, which better meets the most compact packing principle to a certain extent, and improves the degree of product densification. In addition, bimodal alumina has higher reactivity, participates in the reaction to generate spinel phase under medium temperature conditions, and promotes product sintering.
[0019] The present invention selects AlSi12 alloy with Si content of 11%, Al-Mg alloy with Al content of 47% and boron carbide as reaction precursors, wherein the AlSi12 alloy improves the product's resistance to molten steel erosion and increases the product's service life; the magnesium-aluminum alloy can participate in the generation of MgAlON structural reaction intermediates; boron carbide is introduced as a carbide, which has a large wetting angle with oxide slag and poor wettability, and can improve the product's resistance to slag erosion. The combination of the three has the following advantages: (1) When high-temperature sintering is carried out in a nitrogen atmosphere with a low oxygen partial pressure, as the temperature rises, metal Al can react to form AlN and Al2O. After metal Mg is vaporized, it participates in the formation of MgAlON phase in the matrix, greatly improving the corrosion resistance and thermal stability of the refractory bricks, thereby extending the service life; (2) The present invention uses AlSi12 alloy and Al-Mg alloy instead of directly using magnesium and aluminum. This is because aluminum and magnesium are highly active and easily form a dense oxide film on the surface under normal temperature conditions, which is not conducive to the subsequent formation of aluminum nitride or aluminum carbide, the subsequent reaction, and the formation of MgAlON structure. The high reaction starting temperature of the alloy is more conducive to the formation of MgAlON structure.
[0020] The binder is any one of the following: phenolic resin, a mixture of phenolic resin and magnesium aluminum gel at a mass percentage of 1:0.43, and a mixture of magnesium aluminum gel dry powder and deionized water at a mass percentage of 1:0.3. Among them, the viscosity of the phenolic resin is 22000-24000MPa﹒s, and the residual carbon content is 6%. Selecting a high-viscosity (viscosity of 22000-24000MPa﹒s) phenolic resin with a residual carbon content of about 6% as a binder can improve the product's room temperature performance and does not participate in the matrix reaction under service conditions. Selecting nano-scale magnesium aluminum gel dry powder, using the nano effect and its ultra-high reactivity, promotes product sintering.
[0021] The high-temperature firing of fired bricks is carried out in a nitrogen atmosphere. In the nitrogen-dominated reducing atmosphere, the metal aluminum in the brick matrix is partially nitrided to form AlN, and part of it is incompletely oxidized to form Al2O due to the low oxygen partial pressure. The overall reaction equation is as follows: AlN(g)+3Al2O(g)+7Mg(g)+3N2(g)+2O2(g)→7MgAlON(s) AlON(g)+Mg(g)→MgAlON(s) Among them, the MgAlON structure is crisscrossed and woven in the cavity inside the refractory bricks, forming a dense, erosion-resistant and permeable layer, which greatly improves product performance.
[0022] Beneficial effects: 1) The specific supply form of the refractory bricks of the present invention is determined according to the actual working conditions. It can be supplied by unfired bricks that are only subjected to baking operations, or by fired bricks that are fired into fired bricks through high-temperature firing operations in a nitrogen atmosphere. Among them, when the on-site working conditions are rough vacuum (<53Pa) and the smelting temperature is higher than 1700°C, unfired bricks are used for supply, otherwise fired bricks are required for supply. The ultimate goal is to create an environment that is more suitable for the development of MgAlON structure. Determining whether to supply fired bricks or unfired bricks is ultimately determined based on actual working conditions, which can reduce product energy consumption to a certain extent and meet the concept of green and sustainable development.
[0023] 2) The fired bricks of the present invention are fired at high temperature under nitrogen protection. The refractory bricks combined with the MgAlON structure have higher high temperature resistance and stability, and can adapt to a wider range of smelting process requirements.
[0024] 3) When the binder of the refractory bricks of the present invention is a mixture of phenolic resin and magnesium aluminum gel, a smoke-generating and environmentally friendly baking system can be adopted to meet the concept of green and sustainable development.
[0025] 4) The refractory bricks of the present invention can effectively improve the production efficiency and quality of steel smelting, thereby making steel smelting more environmentally friendly, energy-saving, safe and sustainable. Compared with the prior art, the new refractory bricks have higher performance and a wider range of applications. At the same time, the preparation process is more optimized, which can effectively improve production efficiency and quality, reduce production costs, and have obvious advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the microstructure diagram of the unfired brick prepared in Example 1 after being used in a steelmaking furnace. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] For the RH slag system of a steel plant, the amount of fused spinel added was adjusted.
[0030] In order to prepare refractory bricks with better refractory performance, the preparation method of refractory bricks in this embodiment is as follows: Step 1, raw material processing: weigh the raw materials according to the mass percentage in Table 1, put large crystalline fused magnesia, coarse dicalcium fused magnesia, fused spinel, sintered spinel, bimodal alumina, AlSi12 alloy and Al-Mg alloy in a blender according to the mass percentage and stir evenly to obtain a granular mixture; Place fine dicalcium fused magnesia sand and boron carbide in a mixer and stir evenly to obtain a fine powder mixture; Step 2: Add a binder to the granular mixture and mix them evenly, then add the fine powder mixture and mix them evenly to obtain a mud material; Step 3: Treat the mud material for 3-4 days; Step 4: Place the clay material in a mixer, add a binder depending on the bonding conditions of the clay material, stir and mix to obtain a mixed material; Step 5: High pressure molding the mixed material under a pressure of 1000T to obtain a brick; Step six: Place the bricks in a drying oven for baking, first keep them at 100°C for 8 hours, then keep them at 200°C for 16 hours, so that the refractory bricks are fully dried, their room temperature strength and resistance to slag erosion are improved, and unfired bricks are obtained.
[0031] Table 1 Raw materials used in Example 1
[0032] Figure 1 The figure shows the microstructure of the unburned bricks prepared in this embodiment after being used in a steelmaking furnace. It can be seen from the figure that there are many flaky MgAlON structures (as indicated by the arrows) crisscrossed inside the bricks, which can improve the corrosion resistance of the refractory bricks.
[0033] The room temperature compressive strength of the refractory bricks obtained in this example is 120 MPa and the bulk density is 3.15 g / cm 3 The prepared refractory bricks are used in the industrial production of smelting high-quality low-sulfur steel. This product has been used in the RH furnace of the steel plant. The lower trough furnace can reach a maximum of 476 times, and the circulating pipe immersion pipe can reach a maximum of 147 times.
[0034] Example 2
[0035] For the LF slag system of a steel plant, magnesium-aluminum gel was selected as a binder to control the firing atmosphere and temperature.
[0036] In order to prepare refractory bricks with better refractory performance, this embodiment adopts the following method: Step 1, raw material processing: weigh the raw materials according to the mass percentage in Table 2, put large crystalline fused magnesia, coarse dicalcium fused magnesia, fused spinel, sintered spinel, bimodal alumina, AlSi12 alloy and Al-Mg alloy in a blender according to the mass percentage and stir evenly to obtain a granular mixture; Place fine dicalcium fused magnesia sand and boron carbide in a mixer and stir evenly to obtain a fine powder mixture; Step 2: Add a binder to the granular mixture and mix them evenly, then add the fine powder mixture and mix them evenly to obtain a mud material; Step 3: Treat the mud material for 3-4 days; Step 4: Place the clay material in a mixer, add a binder depending on the bonding conditions of the clay material, stir and mix to obtain a mixed material; Step 5: High pressure molding the mixed material under a pressure of 2000T to obtain a brick; Step 6: Place the bricks in a drying oven for baking, and keep them at 110°C for 24 hours to fully dry the refractory bricks;
[0037] Step 7: Place the completely dried refractory bricks into a sagger and fire them in a nitrogen protective atmosphere at a maximum firing temperature of 1700°C for 2 hours to promote the formation of MgAlON structure in the green matrix, thereby obtaining fired bricks.
[0038] Table 2 Raw materials used in Example 2
[0039] The refractory bricks obtained in this example have a mass density of 130 MPa and a bulk density of 3.12 g / cm 3 The prepared refractory bricks are used in the industrial production of smelting high-quality low-sulfur steel grades. This product has been used in the LF furnace of the steel plant, and customers have given high feedback on satisfaction.
[0040] Example 3
[0041] For the LF slag system of a certain steel plant, phenolic resin + magnesium aluminum gel was selected as a binder and the drying system was adjusted.
[0042] In order to prepare refractory bricks with better refractory performance, this embodiment adopts the following method: Step 1, raw material processing: weigh the raw materials according to the mass percentage in Table 3, put large crystalline fused magnesia, coarse dicalcium fused magnesia, fused spinel, sintered spinel, bimodal alumina, AlSi12 alloy and Al-Mg alloy in a blender according to the mass percentage and stir evenly to obtain a granular mixture; Place fine dicalcium fused magnesia sand and boron carbide in a mixer and stir evenly to obtain a fine powder mixture; Step 2: Add a binder to the granular mixture and mix them evenly, then add the fine powder mixture and mix them evenly to obtain a mud material; Step 3: Treat the mud material for 3-4 days; Step 4: Place the clay material in a mixer, add a binder according to the bonding conditions of the clay material, stir and mix to obtain a mixed material; Step 5: High pressure molding the mixed material under a pressure of 2500T to obtain a brick;
[0043] Step 6: Place the bricks in a drying oven for baking and keep them at 350°C for 16 hours to fully dry the refractory bricks, improve their room temperature strength and resistance to slag erosion, and obtain unburned bricks.
[0044] Table 3 Raw materials used in Example 3
[0045] The refractory bricks obtained in this example have a bulk density of 3.15 g / cm 3 The prepared refractory bricks are used in the industrial production of smelting high-quality low-sulfur steel. This product has been used in the LF furnace of a steel plant, and customers have reported that the on-site use environment has been improved.
[0046] It should be noted that in the process of preparing refractory bricks in Examples 1-3, during the mixing in step 4, an appropriate amount of binder can be added according to the state of the clay to improve the molding performance of the clay. However, the total amount of binder added in steps 2 and 4 is 3-7% of the mass of the refractory bricks.
[0047] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any equivalent changes or modifications made according to the essence of the present invention should be included in the protection scope of the present invention.
Claims
1. A refractory brick for steelmaking furnace lining, characterized in that: The components and their mass percentages are: Large crystal fused magnesia 35~40%; Coarse dicalcium fused magnesia 20~25%; Fine dicalcium fused magnesia 15-20%; Fused spinel 4~8%; Sintered spinel 4~8%; Bimodal alumina 4~8%; AlSi12 alloy 5~10%; Al-Mg alloy 2~5%; Boron carbide 2~5%; The sum of the mass percentages of each component is 100%.
2. The refractory brick for steelmaking furnace lining according to claim 1, characterized in that: The refractory bricks also contain a binder accounting for 3-7% of the total mass of the refractory bricks, and the binder is any one of the following: (a) phenolic resin; (ii) phenolic resin and magnesium aluminum gel are mixed in a mass percentage of 1:0.43; (iii) mixing magnesium aluminum gel dry powder and deionized water in a mass percentage of 1:0.3; The viscosity of the phenolic resin used in (i) and (ii) is 22000-24000 MPa﹒ s, and the residual carbon content is 6%; The magnesium aluminum gel used in (ii) is prepared by mixing magnesium aluminum gel dry powder and water in a mass ratio of 1:0.18, and the particle size of the magnesium aluminum gel dry powder is less than 100 nm.
3. The refractory brick for steelmaking furnace lining according to claim 1, characterized in that: The particle size of large crystal fused magnesia is 4~1mm; The particle size of coarse dicalcium fused magnesia is 1-0mm; The particle size of fine dicalcium fused magnesia is 200 mesh; Fused spinel 5μm; Sintered spinel 2-5μm; Bimodal alumina 5μm; AlSi12 alloy 10μm; Al-Mg alloy 100 μm; Boron carbide 350 mesh.
4. The refractory brick for steelmaking furnace lining according to claim 1, characterized in that: In large crystal fused magnesia, the content of periclase is >97%; In dicalcium fused magnesia, the content of MgO is 96-99%, and the ratio of impurity phase CaO to SiO2 is 2; In fused spinel, the MgO content is >78%; Bimodal alumina is an activated alumina powder with a bimodal distribution of particle size; In sintered spinel, the Al2O3 content is greater than 76%; In Al-Mg alloy, the Al content is greater than 47%.
5. A method for preparing refractory bricks for steelmaking furnace lining, characterized in that: The main steps are as follows: Step 1, placing large crystalline fused magnesia, coarse dicalcium fused magnesia, fused spinel, sintered spinel, bimodal alumina, AlSi12 alloy and Al-Mg alloy in a blender according to mass percentage and stirring evenly to obtain a granular mixture; Place fine dicalcium fused magnesia sand and boron carbide in a mixer and stir evenly to obtain a fine powder mixture; Step 2: Add a binder to the granular mixture and mix them evenly, then add the fine powder mixture and mix them evenly to obtain a mud material; Step 3, treating the mud material; Step 4: placing the clay material in a mixer, stirring and mixing to obtain a mixed material; Step 5: High pressure forming the mixed material under a pressure of 630T~2500T to obtain a brick; Step 6: Baking the bricks to obtain refractory bricks.
6. The method for preparing refractory bricks for steelmaking furnace lining according to claim 5, characterized in that: In step three, the material is trapped for 3-4 days.
7. The method for preparing refractory bricks for steelmaking furnace lining according to claim 5, characterized in that: In step 4, during the stirring and mixing process, 0-5% of a binder is added according to the binding conditions of the clay materials. The total amount of the binder added in step 2 and step 4 accounts for 3-7% of the total mass of the refractory bricks.
8. The refractory brick for steelmaking furnace lining according to claim 7, characterized in that: The binder is any one of the following: (a) phenolic resin; (ii) phenolic resin and magnesium aluminum gel are mixed in a mass percentage of 1:0.43; (iii) mixing magnesium aluminum gel dry powder and deionized water in a mass percentage of 1:0.3; The viscosity of the phenolic resin used in (i) and (ii) is 22000-24000 MPa﹒ s, and the residual carbon content is 6%; The magnesium aluminum gel used in (ii) is prepared by mixing magnesium aluminum gel dry powder and water in a mass ratio of 1:0.18, and the particle size of the magnesium aluminum gel dry powder is less than 100 nm.
9. The method for preparing refractory bricks for steelmaking furnace lining according to claim 8, characterized in that: The baking parameters vary depending on the binder added, including: Case 1: When the binder is phenolic resin, the baking parameters are: 80-100℃ for 8 hours in air atmosphere and 190-200℃ for 16 hours; Case 2: When the binder is a mixture of phenolic resin and magnesium aluminum gel, the baking parameters are: 330-350℃ for 16 hours in air atmosphere; Case 3: When the binder is a mixture of magnesium aluminum gel dry powder and deionized water, the baking parameters are: 100-110°C for 24 hours in an air atmosphere.
10. The method for preparing refractory bricks for steelmaking furnace lining according to claim 5, characterized in that: The refractory bricks obtained in step six are subjected to high temperature firing operation in a nitrogen atmosphere, the firing temperature of the high temperature firing operation is 1600-1750°C, and the insulation time is 1-3h.
Citation Information
Patent Citations
Furnace bottom ramming material of RH refining furnace
CN104177102A
Fused magnesia-calcium brick
CN107540390A
Preparation method of calcium-containing periclase-magnesium aluminate spinel refractory material for RH refining furnace
CN114276124A
Alumina-carbon unfired brick for lining molten metal holding furnace, method for producing the same, and furnace equipment and construction method using the same
JP2012036064A
Refractory brick
US20090286668A1