Ceramic proton exchange membrane for microbial fuel cell and preparation method of ceramic proton exchange membrane

By using modifiers such as clay, alumina, and silica to prepare ceramic proton exchange membranes in microbial fuel cells, the problems of high cost and poor mechanical strength of perfluorosulfonic acid membranes were solved, thereby improving the power generation performance and stability of microbial fuel cells.

CN118908745AActive Publication Date: 2024-11-08CENT SOUTH UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410948764.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing perfluorosulfonic acid membranes used as proton exchange membranes in microbial fuel cells suffer from high cost, poor mechanical strength, and severe membrane fouling, which limits their large-scale application and recycling.

Method used

Ceramic proton exchange membranes were prepared by ball milling, granulation, tableting, and calcination using clay, alumina, and silica as inorganic modifiers, and wheat flour, biochar powder, straw powder, and bamboo powder as organic modifiers, thereby optimizing the pore structure and mechanical strength.

Benefits of technology

The prepared ceramic proton exchange membrane has good mass transfer performance, low internal resistance and high mechanical strength, which improves the power generation performance and stability of microbial fuel cells and realizes the replacement of perfluorosulfonic acid membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908745A_ABST
    Figure CN118908745A_ABST
Patent Text Reader

Abstract

The invention provides a ceramic proton exchange membrane for a microbial fuel cell and a preparation method thereof, and the preparation method comprises the following steps: mixing clay, an inorganic modifier and an organic modifier to obtain solid powder; the inorganic modifier is aluminum oxide and silicon dioxide, and the organic modifier is selected from one or more of wheat flour, charcoal powder, straw powder and bamboo powder; and carrying out ball milling, granulation, tabletting and calcination on the solid powder to obtain the ceramic proton exchange membrane. Aiming at the problems that a traditional pure clay ceramic membrane is poor in mass transfer performance, low in electricity generation performance and the like, clay serves as a matrix material, the pore structure of the material is adjusted through a specific inorganic modifier and an organic modifier, and then the novel ceramic proton exchange membrane is prepared through ball milling, granulation, tabletting and calcination. The electrode has the advantages of low manufacturing cost, good proton transmission efficiency and extremely low internal resistance, and can obtain higher output voltage and more stable electricity generation performance when being applied to the microbial fuel cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel cells, and in particular to a ceramic proton exchange membrane for a microbial fuel cell and a preparation method thereof. Background Art

[0002] Microbial fuel cells are a bioelectrochemical system that uses microorganisms to degrade organic waste to produce electrochemical reactions. A typical dual-chamber microbial fuel cell consists of a separate anode and cathode chamber, separated by a proton exchange membrane. Microbial fuel cells have good application prospects in wastewater treatment and energy regeneration. Existing studies have mostly used perfluorosulfonic acid membranes as proton exchange membranes to assemble microbial fuel cells. However, perfluorosulfonic acid membranes have disadvantages such as high cost, poor mechanical strength, and severe membrane contamination, which limit the large-scale application and recycling of microbial fuel cells.

[0003] Ceramic-based proton exchange membranes have become the main choice to replace traditional proton exchange membranes due to their easy-to-control composition, low manufacturing cost, high mechanical strength, and environmental friendliness. Therefore, preparing ceramic membranes with high mass transfer performance is an important way to improve the power generation performance and cycle stability of microbial fuel cells and reduce their operating costs. Summary of the invention

[0004] Based on this, the present invention provides a method for preparing a ceramic proton exchange membrane with good mass transfer performance and high mechanical strength.

[0005] A method for preparing a ceramic proton exchange membrane for a microbial fuel cell comprises the following steps:

[0006] Mixing clay, an inorganic modifier and an organic modifier to obtain a solid powder; the inorganic modifier is alumina and silica, and the organic modifier is selected from one or more of wheat flour, biochar powder, straw powder and bamboo powder; the mass percentage of the alumina in the solid powder is 5% to 15%, the mass percentage of the silica in the solid powder is 5% to 15%, and the mass percentage of the organic modifier in the solid powder is 5% to 15%;

[0007] The solid powder is ball-milled, granulated, tableted and calcined to obtain the ceramic proton exchange membrane.

[0008] In one embodiment, the mass percentage of the aluminum oxide in the solid powder is 9% to 11%, the mass percentage of the silicon dioxide in the solid powder is 9% to 11%, and the mass percentage of the organic modifier in the solid powder is 9% to 11%.

[0009] In one embodiment, the ball milling comprises the following steps: mixing the solid powder with a dispersant, and ball milling at a rotation speed of 200 to 400 r / min for 60 to 120 min.

[0010] Preferably, the dispersant is anhydrous ethanol, and the solid-liquid ratio of the solid powder to the anhydrous ethanol is 0.5 to 2 g / mL. Preferably, the clay is natural clay.

[0011] In one of the embodiments, 2 mm, 3 mm and 5 mm agate grinding balls are added during the ball milling process, and the mass ratio is 12:3:1, and the direction is changed every 30 minutes at a set speed.

[0012] In one embodiment, the granulation comprises the following steps: drying the product after the ball milling, adding a binder for granulation, and screening with a sieve to retain particles with a mesh size of 40 to 60.

[0013] Preferably, the binder is a 5wt% polyvinyl alcohol aqueous solution, and the amount added is 0.5-1.5mL of the binder per 10g of the solid powder. Preferably, the drying temperature is 65-75°C, and the drying time is 0.5-2h.

[0014] In one embodiment, the tableting comprises the following steps: placing the granulated product into a mold, and tableting to obtain a rough embryonic membrane sheet with a thickness of 3 to 6 mm.

[0015] Preferably, the mold is a cylindrical mold, and the diameter is selected according to the actual device of the microbial fuel cell.

[0016] In one embodiment, the tableting is performed using an oil-sealed tablet press, maintaining the pressure at 10 to 15 MPa for 3 to 15 minutes, and then slowly releasing the pressure.

[0017] In one embodiment, the calcination comprises the following steps: calcining the tabletted product under the following temperature increase program: from room temperature to 100-106°C at a rate of 1-2°C / min and keeping the temperature for 30-60min, then to 500°C at a rate of 1-2°C / min and keeping the temperature for 60-120min, and finally to 700-1000°C at a rate of 5-10°C / min and keeping the temperature for 120-180min. Preferably, finally, the temperature is increased to 700-800°C at a rate of 5-10°C / min and kept for 120-180min, more preferably 750°C.

[0018] The present invention also provides a ceramic proton exchange membrane for a microbial fuel cell, which is prepared according to the above preparation method.

[0019] The present invention also provides a microbial fuel cell, which comprises an anode chamber, a cathode chamber and the above ceramic proton exchange membrane.

[0020] The above solution of the present invention has the following beneficial effects:

[0021] The present invention aims at the problems of poor mass transfer performance and low power generation performance of traditional pure clay ceramic membranes. Clay is used as a matrix material, and the pore structure of the material is adjusted by specific inorganic modifiers and organic modifiers, and then a new type of ceramic proton exchange membrane is prepared through ball milling, granulation, tableting and calcination. The ceramic proton exchange membrane can be modified by alumina and silica to have a continuous proton transfer ability, and the organic modifier can optimize the pore size and pore size distribution during the high-temperature carbonization process, thereby improving the water absorption performance of the ceramic proton exchange membrane and improving the pore structure of the ceramic membrane. Therefore, the ceramic proton exchange membrane prepared by the present invention has low manufacturing cost, good proton transfer efficiency and extremely low internal resistance, good water absorption and porosity, and high mechanical strength. It can be applied to microbial fuel cells to replace traditional perfluorosulfonic acid membranes, obtain higher output voltage and lower transfer resistance, effectively improve the power generation performance of microbial fuel cells, and is conducive to the large-scale application of microbial fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a surface microscopic morphology of the ceramic proton exchange membrane prepared in Example 1 of the present invention;

[0023] Figure 2 is the output voltage of the ceramic membrane microbial fuel cell in Example 2 of the present invention;

[0024] Figure 3 is the AC impedance spectrum of the ceramic membrane microbial fuel cell in Example 2 of the present invention;

[0025] Figure 4 The power density and polarization curve of the ceramic membrane microbial fuel cell in Example 2 of the present invention. DETAILED DESCRIPTION

[0026] In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. The reagents and instruments used in the examples are conventionally selected in the art unless otherwise specified. The experimental methods without specific conditions in the examples are implemented according to conventional conditions, such as the conditions described in the literature, books or methods recommended by the manufacturer.

[0028] Example 1

[0029] The ceramic proton exchange membrane is prepared by the following method:

[0030] 1. Preparation of ceramic proton exchange membrane precursor

[0031] (a) Ball milling

[0032] Weigh an appropriate amount of natural clay, silica, alumina, and wheat flour in a mass ratio of 7:1:1:1 and place them in an agate ball mill. Add anhydrous ethanol as a dispersing solvent at a solid-liquid ratio of 1:1 (1 mL of anhydrous ethanol per 1 g of solid), and add agate grinding balls in a ratio of 2 mm: 3 mm: 5 mm = 12:3:1. Set the speed to 400 r / min, change the direction every 30 minutes, and the total ball milling time is 120 minutes.

[0033] (b) Grinding and granulation

[0034] The mixture obtained after ball milling was placed in an oven and dried at 70°C for 60 minutes. The mixture powder obtained after drying was granulated, and a 5% polyvinyl alcohol solution was used as a binder. 1 mL of the binder was added to every 10 g of the raw material, and the mixture was ground and granulated in a mortar. The mixture was sieved with a 40-60 mesh screen, and particles with a size between 40 and 60 mesh were retained.

[0035] 2. Preparation of ceramic proton exchange membrane

[0036] (a) Tablet molding

[0037] Weigh 8g of particles with a size between 40 and 60 meshes and put them into a cylindrical mold with a diameter of 5mm. Use an oil-sealed tablet press to maintain the pressure at 14MPa for 10 minutes, then slowly release the pressure to obtain a 4mm rough film.

[0038] (b) High temperature calcination

[0039] The rough membrane obtained by pressing is placed in a digital temperature-controlled muffle furnace. First, the temperature is raised to 106°C at 2°C / min and kept for 30 minutes to remove moisture, then the temperature is raised to 500°C at 1°C / min and kept for 120 minutes to remove plastic, and finally the temperature is raised to 750°C at 5°C / min and kept for 180 minutes to calcine and shape, and finally the finished ceramic proton exchange membrane is obtained.

[0040] Figure 1 This is a scanning electron microscope image of the surface of the ceramic proton exchange membrane prepared in this embodiment. From the microscopic morphology, it can be seen that a micron-level pore distribution is formed on the surface of the ceramic membrane, which improves the porosity and water absorption capacity of the ceramic membrane itself. In addition, more porosity can increase the contact rate between the silicon-aluminum group and the proton in the ceramic membrane, thereby improving the proton transmission capacity of the ceramic membrane. In this embodiment, the addition of wheat flour optimizes the pore structure of the ceramic membrane, and the addition of silicon-aluminum oxide enables the ceramic membrane to form more adsorbed proton groups, thereby optimizing the proton transmission efficiency of the ceramic membrane. At the same time, the addition of silicon-aluminum oxide also forms a complex spatial structure of stacked crystalline particles on the surface of the clay-based ceramic proton exchange membrane, and this structure gives the ceramic membrane stable mechanical strength.

[0041] Example 2 Construction of a dual-chamber microbial fuel cell

[0042] The clay-based ceramic proton exchange membrane prepared in Example 1 was applied to a dual-chamber microbial fuel cell. The specific structure of the dual-chamber microbial fuel cell constructed includes: (1) a 1000Ω resistor; (2) a conductor; (3) a clay-based ceramic proton exchange membrane; (4) a carbon felt electrode with a size of 3 cm×3 cm (length×width). 10 g of activated sludge and 120 mL of simulated wastewater were placed in the anode chamber, wherein the composition of the simulated wastewater was: 0.2 g / L ammonium chloride, 0.075 g / L calcium chloride dihydrate, 0.33 g / L potassium chloride, 0.30 g / L sodium chloride, 0.315 g / L magnesium chloride, 1.26 g / L dipotassium hydrogen phosphate, 0.42 g / L potassium dihydrogen phosphate, 1 mL / L trace element solution, 1 g / L yeast extract, and 3.29 g / L sodium acetate. The cathode chamber is filled with 50mM PBS-potassium ferrocyanide solution, which consists of 0.13g / L potassium chloride, 0.31g / L ammonium chloride, 2.77g / L sodium dihydrogen phosphate dihydrate, 11.54g / L disodium hydrogen phosphate dodecahydrate, and 16.45g / L potassium ferrocyanide. The trace elements include: Fe, Zn, Mn, Mo, Co, and Ni. The external circuit of the double-chamber microbial fuel cell is connected to a 1000Ω resistor, and the battery output voltage is recorded regularly to draw a curve of voltage change over time. Figure 2 As far as we know, the dual-chamber microbial fuel cell operates stably for multiple consecutive cycles, with the highest operating voltage exceeding 600mV, and has a good power generation effect.

[0043] (1) AC impedance measurement of a two-chamber microbial fuel cell constructed with a clay-based ceramic proton exchange membrane

[0044] The electrochemical performance test of the anode of the microbial fuel cell was carried out on the Donghua DH7000 electrochemical workstation. The electrochemical impedance spectroscopy (EIS) test was carried out using the double-chamber microbial fuel cell anode, using a three-electrode system, in which the anode was the working electrode, the cathode was the counter electrode, and the silver-silver chloride electrode was the reference electrode.

[0045] Figure 3 The AC impedance spectrum of the constructed dual-chamber microbial fuel cell. Using the ZView software and the fuel cell equivalent circuit fitting calculation, the battery solution resistance is 1.5Ω, the anode charge transfer resistance is 7.9Ω, the cathode charge transfer resistance is 18.8Ω, the cathode diffusion resistance is 104Ω, and the fitting total internal resistance is 132.2Ω. The modifier fully adjusts the pore structure of the ceramic membrane, making it have excellent mass transfer efficiency. When the ceramic membrane is used as the proton exchange membrane of the microbial fuel cell, the resistance of proton transfer from the anode chamber to the cathode chamber is low, thereby enhancing the power generation performance of the microbial fuel cell.

[0046] (2) Polarization curve and power density

[0047] By changing the external resistance (9k, 8k, 7k, 6k, 5k, 4k, 3k, 2k, 1.8k, 1.6k, 1.4k, 1.2k, 1k, 900, 800, 700, 600, 500, 400, 300, 200, 100, 90, 80, 70, 60, 50, 40Ω) and testing the output voltage and current of the battery, the polarization curve can be obtained and the power density of the battery can be calculated. Figure 4 As shown in Figure 2, when ceramic membrane is used as proton exchange membrane, the maximum power density of microbial fuel cell can reach 421.7 mW.m -2 , the corresponding current density is 765.3mA.m -2 , showing good electrochemical properties and power generation performance.

[0048] Example 3

[0049] In this example, the wheat flour in Example 1 was replaced with biochar powder, straw powder, and bamboo powder, respectively, and performance tests were performed in the manner of Example 2. The results are shown in the following table.

[0050] Group Fitting total internal resistance Maximum power density Corresponding current density Biochar powder 410.4Ω <![CDATA[170.2mW.m -2 ]]> <![CDATA[640.3mA.m -2 ]]> Straw powder 705.6Ω <![CDATA[361.2mW.m -2 ]]> <![CDATA[708.3mA.m -2 ]]> Bamboo powder 625.0Ω <![CDATA[372.5mW.m -2 ]]> <![CDATA[722.5mW.m -2 ]]>

[0051] Comparative Example 1

[0052] This comparative example is substantially the same as Example 1, except that no wheat flour is added, and natural clay, silicon dioxide and aluminum oxide are mixed in a mass ratio of 8:1:1.

[0053] Comparative Example 2

[0054] This comparative example is substantially the same as Example 1, except that no alumina is added, and natural clay, silicon dioxide and wheat flour are mixed in a mass ratio of 7:2:1.

[0055] Comparative Example 3

[0056] This comparative example is basically the same as Example 1, except that wheat flour is replaced with maltose powder, and natural clay, silicon dioxide, aluminum oxide and maltose powder are mixed in a mass ratio of 7:1:1:1.

[0057] The above comparative example was tested for the fitted total internal resistance, maximum power density and maximum current density in the manner of Example 2. The results are shown in the following table. It can be seen that the microbial fuel cell prepared by the ceramic proton exchange membrane is obviously inferior to that of Example 1.

[0058] Group Fitting total internal resistance Maximum power density Corresponding current density Comparative Example 1 1457Ω <![CDATA[316.0mW.m -2 ]]> <![CDATA[662.5mA.m -2 ]]> Comparative Example 2 362.2Ω <![CDATA[345.4mW.m -2 ]]> <![CDATA[692.3mA.m -2 ]]> Comparative Example 3 322.0Ω <![CDATA[151.1mW.m -2 ]]> <![CDATA[601.2mA.m -2 ]]>

[0059] Example 4 Optimization of the addition ratio of alumina and silica

[0060] As shown in the table below, the mass ratio of natural clay, silica, alumina and wheat flour was adjusted, and then the fitted total internal resistance, maximum power density and maximum current density were detected as described in Example 2. It can be seen that the preferred addition ratios of alumina, silica and wheat flour are all about 10%.

[0061] Mass ratio of natural clay, silica, alumina and wheat flour Fitting total internal resistance Maximum power density Corresponding current density 7:1:1:1 132.2Ω <![CDATA[421.7mW.m -2 ]]> <![CDATA[765.3mA.m -2 ]]> 7:0.5:1.5:1 182.1Ω <![CDATA[400.3mW.m -2 ]]> <![CDATA[735.2mA.m -2 ]]> 7:1.5:0.5:1 237.0Ω <![CDATA[362.7mW.m -2 ]]> <![CDATA[709.7mA.m -2 ]]>

[0062] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a ceramic proton exchange membrane for a microbial fuel cell, It is characterized in that The following steps are involved: Mixing clay, an inorganic modifier and an organic modifier to obtain a solid powder; the inorganic modifier is alumina and silica, and the organic modifier is selected from one or more of wheat flour, biochar powder, straw powder and bamboo powder; the mass percentage of the alumina in the solid powder is 5% to 15%, the mass percentage of the silica in the solid powder is 5% to 15%, and the mass percentage of the organic modifier in the solid powder is 5% to 15%; The solid powder is ball-milled, granulated, tableted and calcined to obtain the ceramic proton exchange membrane.

2. The preparation method according to claim 1, It is characterized in that The mass percentage of the aluminum oxide in the solid powder is 9% to 11%, the mass percentage of the silicon dioxide in the solid powder is 9% to 11%, and the mass percentage of the organic modifier in the solid powder is 9% to 11%.

3. The preparation method according to claim 1, It is characterized in that The ball milling comprises the following steps: mixing the solid powder with a dispersant, and ball milling for 60 to 120 minutes at a rotation speed of 200 to 400 r / min; the dispersant is anhydrous ethanol, and the solid-liquid ratio of the solid powder to the anhydrous ethanol is 0.5 to 2 g / mL.

4. The preparation method according to claim 3, It is characterized in that During the ball milling process, agate grinding balls of 2 mm, 3 mm and 5 mm were added with a mass ratio of 12:3:1, and the direction of rotation was changed every 30 minutes at a set speed.

5. The preparation method according to claim 1, It is characterized in that The granulation comprises the following steps: drying the product after the ball milling, then adding a binder for granulation, and sieving with a sieve to retain particles with a mesh size of 40 to 60; the binder is a 5wt% polyvinyl alcohol aqueous solution, and the amount added is 0.5 to 1.5 mL of the binder per 10 g of the solid powder.

6. The preparation method according to claim 1, It is characterized in that The tableting process comprises the following steps: placing the granulated product into a mold, and tableting to obtain a rough embryonic membrane sheet with a thickness of 3 to 6 mm.

7. The preparation method according to claim 6, It is characterized in that The tabletting is performed using an oil-sealed tabletting machine, maintaining the pressure at 10-15 MPa for 3-15 minutes, and then slowly releasing the pressure.

8. The preparation method according to claim 1, It is characterized in that The calcination comprises the following steps: calcining the tabletted product under the following temperature increase program: heating from room temperature to 100-106°C at a rate of 1-2°C / min and keeping the temperature for 30-60min, then heating to 500°C at a rate of 1-2°C / min and keeping the temperature for 60-120min, and finally heating to 700-1000°C at a rate of 5-10°C / min and keeping the temperature for 120-180min.

9. A ceramic proton exchange membrane for microbial fuel cells, It is characterized in that Prepared according to the preparation method according to any one of claims 1 to 8.

10. A microbial fuel cell, It is characterized in that It comprises an anode chamber, a cathode chamber and the ceramic proton exchange membrane according to claim 9.

Citation Information

Patent Citations

  • Shaped porous bodies of alpha-alumina and methods for the preparation thereof

    CA2667980A1

  • Preparation method of ceramic fiber reinforced ceramic membrane supporter

    CN104387112A

  • Method for preparing high-toughness porous ceramic membrane supporting body by utilizing microorganisms

    CN108499372A

  • Low-aluminum high-porosity porous ceramic material and preparation method thereof

    CN114057508A

  • Film using denatured clay

    JP2007277078A