Tetra (2-propylheptyl) pyromellitic acid tetra (2-propylheptyl) ester as well as preparation method and application thereof
Tetra(2-propylheptane) esterification reaction of phenylase tetrachloride and 2-propylheptane alcohol was prepared, which solved the problems of high TOTM cost and environmental risks, and provided an environmental protection and cost Low- and high-performance plasticizer, suitable for plastic materials such as PVC, has excellent heat resistance and high volume resistivity.
Patent Information
- Application Number
- CN202410937636.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-08
AI Technical Summary
The existing trioctyl trimellite (TOTM) plasticizers are expensive and have potential risks to ecosystems and human health. The environmental impact of by-products and wastes in their production process is restricted by REACH regulations, which requires an environmental protection, Low-cost, high-performance alternative.
Tetra(2-propylheptyl) phenylalic acid ester was prepared by esterification reaction of phenylalic acid or phenylalic anhydride and 2-propylheptol under the action of titanate catalysts, and was refined by fine purification This ester is obtained as a substitute for plastics such as polyvinyl chloride (PVC).
Tetrakis(2-propylheptane) phenylase has excellent heat resistance and conductivity, low cost, simple synthesis process, suitable for industrial processing, replaces expensive TOTM, and reduces environmental risks, suitable for high Standard industries such as the avionics wire field.
Smart Images

Figure CN118908831A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer chemical synthesis, in particular to tetra(2-propylheptyl)pyromellitic acid ester, a preparation method and application thereof. Background Art
[0002] Trioctyl trimellitate, abbreviated as TOTM, also known as tri(2-ethylhexyl) trimellitate, is an excellent plasticizer with low volatility, good heat resistance, minimal migration, electrical insulation, durability, low toxicity, water resistance, and suitable compatibility. It is primarily used in plastic products such as polyvinyl chloride (PVC), vinyl chloride copolymers, nitrocellulose, and ethyl cellulose. It is also used in heat-resistant wire and cable materials, plates, sheets, and gaskets.
[0003] In terms of production methods, TOTM is usually produced through esterification reaction using trimellitic anhydride (TMA) and octanol as raw materials. During the preparation process, concentrated sulfuric acid, solid acid, metal oxides, etc. are used as catalysts, and the final product is obtained through purification processes such as neutralization, water washing, decolorization, and dealcoholization.
[0004] However, TMA's increasing price and the inconvenience of transportation and use caused by its easy sublimation have resulted in higher costs for TOTM than traditional plasticizers, directly impacting its competitiveness in price-sensitive markets. Furthermore, while TMA itself is non-toxic and environmentally friendly, the byproducts and waste generated during its production, as well as its persistence and bioaccumulation in the environment, pose potential risks to ecosystems and human health. It is currently restricted under REACH (Registration, Evaluation, Authorisation and Restriction of Chemicals), a European Union regulation governing chemicals.
[0005] Therefore, developing TOTM substitutes and alternative technologies to provide an environmentally friendly, low-cost, high-performance plasticizer is a technical problem that needs to be solved urgently. Summary of the Invention
[0006] In order to overcome the deficiencies of the prior art, one of the objects of the present invention is to provide tetra(2-propylheptyl)pyromellitate.
[0007] A second object of the present invention is to provide a method for preparing tetra(2-propylheptyl)pyromellitic acid.
[0008] A third object of the present invention is to provide an application of tetra(2-propylheptyl)pyromellitic acid in a plasticizer.
[0009] One of the objectives of the present invention is achieved by the following technical solution: a tetrakis(2-propylheptyl)pyromellitic acid ester is obtained by esterification of pyromellitic acid or pyromellitic anhydride with 2-propylheptanol in the presence of a catalyst, wherein the tetrakis(2-propylheptyl)pyromellitic acid ester has the following reaction formula:
[0010]
[0011] Optionally, the molar ratio of pyromellitic acid or pyromellitic anhydride to 2-propylheptanol is 1:(4-6).
[0012] Optionally, the purity of the pyromellitic acid or pyromellitic anhydride is 98.5-99.9%.
[0013] Optionally, the structural formula of the pyromellitic acid is as follows:
[0014] The structural formula of the pyromellitic anhydride is as follows:
[0015] Optionally, the catalyst is selected from a titanate catalyst, and the molar ratio of the catalyst to 2-propylheptanol is 1:(2000-5000).
[0016] Optionally, after the acid value of the esterification reaction reaches 0.3 mgKOH / g, alkali is added to remove excess water and alcohol, and the product is refined and purified to obtain tetra(2-propylheptyl)pyromellitic acid ester.
[0017] The second object of the present invention is achieved by the following technical solution: a method for preparing tetra(2-propylheptyl)pyromellitic acid ester as described above, comprising the following steps:
[0018] (1) adding pyromellitic acid or pyromellitic anhydride and 2-propylheptanol into a reactor, stirring and heating;
[0019] (2) When the temperature reaches 110-130°C, add the catalyst and continue to heat to 180-210°C with stirring to carry out the esterification reaction;
[0020] (3) After the acid value of the esterification reaction reaches 0.3 mgKOH / g, the reaction is terminated;
[0021] (4) Add alkali, remove excess water and excess alcohol, and purify the mixture to obtain tetra(2-propylheptyl)pyromellitic acid tetracarboxylate.
[0022] Optionally, in step (1), the molar ratio of pyromellitic acid or pyromellitic anhydride to 2-propylheptanol is 1:(4-6).
[0023] Optionally, in step (2), the catalyst is selected from a titanate catalyst, and the molar ratio of the catalyst to 2-propylheptanol is 1:(2000-5000).
[0024] The third object of the present invention is achieved by adopting the following technical solution: an application of the above-mentioned tetra(2-propylheptyl)pyromellitic acid ester as a plasticizer in polyvinyl chloride (PVC).
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) There are many types of plasticizers, among which trioctyl trimellitate (TOTM) is expensive and poses potential risks to the ecosystem and human health, and is currently restricted under the REACH regulations. However, the raw materials used in the synthesis process of tetra(2-propylheptyl) pyromellitate of the present invention are safe and low-cost, and the synthesis process and steps are simple, making it suitable for industrial processing and production. It can be used as a substitute for trioctyl trimellitate (TOTM) plasticizer, or even a better improved product.
[0027] (2) In addition, the tetrakis(2-propylheptyl)pyromellitic acid ester of the present invention is compared with the performance of several commonly used plasticizers. The tetrakis(2-propylheptyl)pyromellitic acid ester of the present invention has excellent heat resistance and electrical conductivity. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.
[0029] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used are commercially available or commonly used in the art. The methods in the following examples are all conventional methods in the art unless otherwise specified.
[0030] The tetrakis(2-propylheptyl)pyromellitic acid ester provided by the present invention is obtained by esterification reaction of pyromellitic acid or pyromellitic anhydride with 2-propylheptanol in the presence of a catalyst. The reaction formula of the tetrakis(2-propylheptyl)pyromellitic acid ester is as follows:
[0031]
[0032] As a further embodiment, the molar ratio of pyromellitic acid or pyromellitic anhydride to 2-propylheptanol is 1:(4-6). Pyromellitic acid is selected from, but not limited to, 1,2,4,5-benzenetetracarboxylic acid with product number B4007 provided by Sigma-Aldrich; pyromellitic anhydride is selected from, but not limited to, pyromellitic dianhydride with product number 412287 provided by Sigma-Aldrich; and 2-propylheptanol can be purchased from, for example, BASF of Germany, Degussa, and BASF-YPC of China.
[0033] As a further embodiment, the purity of the pyromellitic acid or pyromellitic anhydride is 98.5-99.9%. In this application, pyromellitic acid or pyromellitic anhydride of different purities as raw materials for the esterification reaction have an impact on the product purity, by-products, and production cost of the reaction process. In terms of raw material price, pyromellitic anhydride with a purity of 99.5% > pyromellitic anhydride with a purity of 98.5% > pyromellitic acid with a purity of 99.5% > pyromellitic acid with a purity of 98.5%.
[0034] As a further embodiment, the structural formula of the pyromellitic acid is as follows:
[0035] The structural formula of the pyromellitic anhydride is as follows:
[0036] As a further embodiment, the catalyst is selected from titanate catalysts, and the molar ratio of the catalyst to 2-propylheptanol is 1:(2000-5000).
[0037] As a further embodiment, after the acid value of the esterification reaction reaches 0.3 mgKOH / g, alkali is added to remove excess water and alcohol, and the product is refined and purified to obtain tetra(2-propylheptyl)pyromellitic acid.
[0038] The present invention also provides a method for preparing tetra(2-propylheptyl)pyromellitic acid ester as described above, comprising the following steps:
[0039] (1) adding pyromellitic acid or pyromellitic anhydride and 2-propylheptanol into a reactor, stirring and heating;
[0040] (2) When the temperature reaches 110-130°C, add the catalyst and continue to heat to 180-210°C with stirring to carry out the esterification reaction;
[0041] (3) After the acid value of the esterification reaction reaches 0.3 mgKOH / g, the reaction is terminated;
[0042] (4) Add alkali, remove excess water and excess alcohol, and purify the mixture to obtain tetra(2-propylheptyl)pyromellitic acid tetracarboxylate.
[0043] As a further embodiment, in step (1), the molar ratio of pyromellitic acid or pyromellitic anhydride to 2-propylheptanol is 1:(4-6).
[0044] As a further embodiment, in step (2), the catalyst is selected from a titanate catalyst, and the molar ratio of the catalyst to 2-propylheptanol is 1:(2000-5000).
[0045] The present invention also provides a use of the above-mentioned tetra(2-propylheptyl)pyromellitic acid ester as a plasticizer in polyvinyl chloride.
[0046] The following are specific embodiments of the present invention. Unless otherwise specified, the raw materials, equipment, etc. used in the following embodiments can be obtained by purchase.
[0047] Example 1
[0048] Tetrakis(2-propylheptyl)pyromellitic acid ester is prepared by the following preparation method, comprising the following steps:
[0049] (1) Pyromellitic acid and 2-propylheptanol are added to a reactor, stirred, and heated; the molar ratio of pyromellitic acid to 2-propylheptanol is 1:4. The purity of the pyromellitic acid is 99.5%.
[0050] (2) When the temperature reaches 110-130° C., a titanate catalyst is added, and the temperature is continued to rise to 180-210° C. with stirring to carry out esterification reaction; the molar ratio of the catalyst to 2-propylheptanol is 1:3000.
[0051] (3) After the acid value of the esterification reaction reaches 0.3 mgKOH / g, the reaction is terminated;
[0052] (4) Add alkali, remove excess water and excess alcohol, and purify the mixture to obtain tetra(2-propylheptyl)pyromellitic acid tetracarboxylate.
[0053] Example 2
[0054] Tetrakis(2-propylheptyl)pyromellitic acid ester is prepared by the following preparation method, comprising the following steps:
[0055] (1) Pyromellitic acid and 2-propylheptanol are added to a reactor, stirred, and heated; the molar ratio of pyromellitic acid to 2-propylheptanol is 1:5. The purity of the pyromellitic acid is 99.5%.
[0056] (2) When the temperature reaches 110-130° C., a titanate catalyst is added, and the temperature is continued to rise to 180-210° C. with stirring to carry out esterification reaction; the molar ratio of the catalyst to 2-propylheptanol is 1:4000.
[0057] (3) After the acid value of the esterification reaction reaches 0.3 mgKOH / g, the reaction is terminated;
[0058] (4) Add alkali, remove excess water and excess alcohol, and purify the mixture to obtain tetra(2-propylheptyl)pyromellitic acid tetracarboxylate.
[0059] Example 3
[0060] Tetrakis(2-propylheptyl)pyromellitic acid ester is prepared by the following preparation method, comprising the following steps:
[0061] (1) Pyromellitic acid and 2-propylheptanol are added to a reactor, stirred, and heated; the molar ratio of pyromellitic acid to 2-propylheptanol is 1:6. The purity of the pyromellitic acid is 99.5%.
[0062] (2) When the temperature reaches 110-130° C., a titanate catalyst is added, and the temperature is continued to rise to 180-210° C. with stirring to carry out esterification reaction; the molar ratio of the catalyst to 2-propylheptanol is 1:5000.
[0063] (3) After the acid value of the esterification reaction reaches 0.3 mgKOH / g, the reaction is terminated;
[0064] (4) Add alkali, remove excess water and excess alcohol, and purify the mixture to obtain tetra(2-propylheptyl)pyromellitic acid tetracarboxylate.
[0065] Example 4
[0066] Tetrakis(2-propylheptyl)pyromellitic acid ester is prepared by the following preparation method, comprising the following steps:
[0067] (1) Pyromellitic anhydride and 2-propylheptanol are added to a reactor, stirred, and heated; the molar ratio of pyromellitic anhydride to 2-propylheptanol is 1:5. The purity of the pyromellitic anhydride is 98.5%.
[0068] (2) When the temperature reaches 110-130° C., a titanate catalyst is added, and the temperature is continued to rise to 180-210° C. with stirring to carry out esterification reaction; the molar ratio of the catalyst to 2-propylheptanol is 1:4000.
[0069] (3) After the acid value of the esterification reaction reaches 0.3 mgKOH / g, the reaction is terminated;
[0070] (4) Add alkali, remove excess water and excess alcohol, and purify the mixture to obtain tetra(2-propylheptyl)pyromellitic acid tetracarboxylate.
[0071] Comparative Example 1
[0072] Compared with the preparation method of Example 2, the difference is that in step (1), the molar ratio of pyromellitic acid to 2-propylheptanol is 1:7, and the other process conditions are the same as those of Example 2.
[0073] Comparative Example 2
[0074] Compared with the preparation method of Example 2, the difference is that in step (1), the molar ratio of pyromellitic acid to 2-propylheptanol is 1:3, and the other process conditions are the same as those of Example 2.
[0075] Effect evaluation and performance testing
[0076] According to the test regulations for ester content, density, volume resistivity, heat resistance level and other properties under HG / T 4889-2016 and UL standards, the properties of tetra(2-propylheptyl)pyromellitic acid in Examples 1-4 and Comparative Examples 1-3 were tested. The test items and results are shown in Table 1.
[0077] Table 1 is the performance test data of tetra(2-propylheptyl)pyromellitic acid ester in various embodiments
[0078]
[0079]
[0080] The synthesis process of tetra(2-propylheptyl)pyromellitic acid ester of the present invention uses safe raw materials, is low-cost, and has simple synthetic processes and steps, making it suitable for industrial processing and production. In addition, the reaction raw materials replace the expensive and environmentally resistant trimellitic anhydride (TMA). The obtained tetra(2-propylheptyl)pyromellitic acid ester has an ester content of greater than 99.5%, is environmentally friendly, and has stable basic properties.
[0081] Tetrakis(2-propylheptyl) pyromellitic acid ester of the present invention can be used as the plasticizer of polyvinyl chloride (PVC) particularly.Tetrakis(2-propylheptyl) pyromellitic acid ester of the present invention can be used alone as the plasticizer of PVC, also can be used together with the conventional plasticizer of this area, and the addition of plasticizer is 1-80% of PVC consumption.For example, can be processed PVC by following component, specifically contain plasticizer 60g, stabilizing agent 3g in every 100 grams of PVC.Wherein, described plasticizer is tetrakis(2-propylheptyl) pyromellitic acid ester of embodiment of the present invention 2, or mentions the mixture of one or more plasticizers of trioctyl trimellitate (TOTM) (as comparative example 3) or di(2-propylheptyl) phthalate) DPHP (as comparative example 4) in background technology.Described stabilizing agent (or claim " stabilizer ") can be lead salt or lead-free calcium zinc, organotin, rare earth etc. types. It will be appreciated by those skilled in the art that the above components and their contents are merely exemplary embodiments, and those skilled in the art may adapt the above components and / or contents to achieve better plasticizing effects based on actual conditions. Table 2 compares the physical properties of tetrakis(2-propylheptyl)pyromellitic acid ester of the present invention with conventional plasticizers. Table 3 compares the properties of processed products of tetrakis(2-propylheptyl)pyromellitic acid ester of the present invention with conventional plasticizers.
[0082] Table 2 Physical properties and cost comparison of tetra(2-propylheptyl)pyromellitic acid ester of the present invention and commonly used plasticizers
[0083]
[0084]
[0085] Table 3 Heat resistance of products processed with tetra(2-propylheptyl)pyromellitic acid ester and common plasticizers of the present invention
[0086] Heat resistance level under UL standard (℃) Example 2 125 Comparative Example 3 (TOTM) 105 Comparative Example 4 (DPHP) 70
[0087] As shown in Table 1-3, tetra(2-propylheptyl)pyromellitate is a specific organic compound used as a plasticizer, particularly in PVC (polyvinyl chloride) plastic products. Tetra(2-propylheptyl)pyromellitate has a high molecular weight, low specific gravity, and a high flash point. A higher molecular weight increases compound stability and migration resistance, while a higher flash point improves chemical safety. Its lower specific gravity allows for lower overall processing costs, leveraging its volumetric cost advantage.
[0088] Compared to existing plasticizers like TOTM and DPHP, tetra(2-propylheptyl)pyromellitate exhibits superior heat resistance, reaching 125°C, the highest heat resistance rating currently offered by any plasticizer. This makes it suitable for use in high-standard industries and fields, such as aviation wiring. Furthermore, the high volume resistivity of tetra(2-propylheptyl)pyromellitate makes it particularly suitable for use in high-temperature wiring technology.
[0089] In summary, the tetra(2-propylheptyl)pyromellitic acid tetracarboxylate of the present invention has excellent heat resistance, high environmental performance and low cost, and can be used as a substitute for TOTM plasticizer, or even a better improved product.
[0090] The above embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and replacements made by technicians in this field on the basis of the present invention fall within the scope of protection required by the present invention.
Claims
1. A tetrakis(2-propylheptyl)pyromellitic acid ester, It is characterized in that It is obtained by esterification reaction of pyromellitic acid or pyromellitic anhydride with 2-propylheptanol in the presence of a catalyst. The structural formula of tetra(2-propylheptyl)pyromellitic acid is as follows:
2. Tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in claim 1, It is characterized in that The molar ratio of the pyromellitic acid or pyromellitic anhydride to 2-propylheptanol is 1:(4-6).
3. Tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in claim 1, It is characterized in that The purity of the pyromellitic acid or pyromellitic anhydride is 98.5-99.9%.
4. Tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in claim 1, It is characterized in that The structural formula of the pyromellitic acid is as follows: The structural formula of the pyromellitic anhydride is as follows:
5. Tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in claim 1, It is characterized in that The catalyst is selected from titanate catalysts, and the molar ratio of the catalyst to 2-propylheptanol is 1:(2000-5000).
6. Tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in claim 1, It is characterized in that After the acid value of the esterification reaction reaches 0.3 mgKOH / g, alkali is added to remove excess water and alcohol, and the mixture is finely purified to obtain tetra(2-propylheptyl)pyromellitic acid.
7. A method for preparing tetrakis(2-propylheptyl)pyromellitic acid ester according to any one of claims 1 to 6, It is characterized in that The steps include: (1) adding pyromellitic acid or pyromellitic anhydride and 2-propylheptanol into a reactor, stirring and heating; (2) When the temperature reaches 110-130°C, add the catalyst and continue to heat to 180-210°C with stirring to carry out esterification reaction; (3) When the acid value of the esterification reaction reaches 0.3 mgKOH / g, the reaction is terminated; (4) adding alkali, removing excess water and excess alcohol, and purifying the mixture to obtain tetra(2-propylheptyl)pyromellitic acid tetracarboxylate.
8. Tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in claim 1, It is characterized in that In step (1), the molar ratio of pyromellitic acid or pyromellitic anhydride to 2-propylheptanol is 1:(4-6).
9. Tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in claim 1, It is characterized in that In step (2), the catalyst is selected from a titanate catalyst, and the molar ratio of the catalyst to 2-propylheptanol is 1:(2000-5000).
10. Use of tetrakis(2-propylheptyl)pyromellitic acid ester as claimed in any one of claims 1 to 9 as a plasticizer in polyvinyl chloride.
Citation Information
Cited By
Tetraisononyl pyromellitic acid ester as well as preparation method and application thereof
CN119431149A
Isooctyl / isononyl / isodecyl pyromellitic acid plasticizer composition as well as preparation method and application thereof
CN119431888A