Sodium carboxymethylcellulose and application thereof

CN118909146APending Publication Date: 2024-11-08CHANGSHU WEIYI TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411136038.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

上述方法存在如下问题:通过与乙二醛发生羟醛缩合反应来制备的速溶型羧甲基纤维素钠,遇到水后乙二醛会重新脱落进入到水中,导致水体中存在乙二醛这样的活性基团,这些残留的活性小分子可能会在后期与其他物质发生化学反应,对最终的产品质量构成安全隐患

Benefits of technology

[0035] By adopting the above technical solution, compared with the existing technology, the benefit of the present invention is that the sodium carboxymethylcellulose of the present invention uses calcium carbonate to perform surface modification on the sodium carboxymethylcellulose, and the process flow is simple. , low cost, while solving the "packing" problem during dissolution and possible product quality and toxicity problems in the later stage, expanding the application field of instant carboxymethylcellulose sodium; the use of matching buffers can avoid the effects of excessive acidification product quality issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005000808660000011
    Figure HDA0005000808660000011
Patent Text Reader

Abstract

The invention discloses sodium carboxymethyl cellulose which is prepared by the following steps: acidifying the surface of sodium carboxymethyl cellulose powder by using a buffer solution, and performing surface calcification modification on the sodium carboxymethyl cellulose by using calcium carbonate, dissolving and uniformly mixing to prepare a buffer solution; in the prepared sodium carboxymethyl cellulose, part of residual calcium carbonate is located between adjacent sodium carboxymethyl cellulose particles, the effect of a disintegrating agent is achieved, and the sodium carboxymethyl cellulose powder is further promoted to be rapidly disintegrated to form a uniform dispersion system. According to the sodium carboxymethyl cellulose disclosed by the invention, the calcium carbonate is adopted for performing surface modification on the sodium carboxymethyl cellulose, so that the process flow is simple, the cost is low, and meanwhile, the problem of core coating during dissolution and the problems of product quality and toxicity possibly existing in the later period are solved; a buffer solution is matched for use, so that the product quality problem caused by excessive acidification is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application date of June 4, 2024, application number 2024107153459, and invention name “Sodium carboxymethyl cellulose, preparation method and application thereof”. Technical Field

[0002] The invention relates to the field of polymer chemical modification, and in particular to a quick-dissolving sodium carboxymethyl cellulose and its application in food additives, cosmetics or coating additives, battery electrode materials and the like. Background Art

[0003] Sodium carboxymethyl cellulose is a modified product of natural polymer compounds. It is widely used in various fields because its aqueous solution has the functions of dispersion, water retention, and viscosity increase. Sodium carboxymethyl cellulose contains a strong polar group-carboxymethyl, which makes the originally water-insoluble cellulose have a strong hydrophilic property, especially when the degree of substitution of the carboxymethyl group is relatively high, its hydrophilic property is even stronger. This type of sodium carboxymethyl cellulose powder will have a "heart-wrapping" phenomenon when poured into the water body, that is, at the moment of contact with water, the surface particles of a small group of powder quickly absorb the surrounding water, forming a water layer with viscosity, and finally forming a complete water layer around the periphery of this group of powder. The existence of the water layer prevents water from quickly penetrating into the powder, making it impossible for the powder to be dissolved by water in a short time, forming a "heart-wrapping" one by one. For the dissolution of the "core", if no measures are taken and it is allowed to dissolve naturally, it will take 10-24 hours, and the viscosity inside the water body is uneven. When the degree of substitution is high, it will take longer. If strong stirring measures are used, it will generally take 1-4 hours to completely dissolve.

[0004] The existence of the "core-wrapping" problem, on the one hand, has imposed some restrictions on the application of sodium carboxymethyl cellulose in certain industries. For example, in the coating industry, sodium carboxymethyl cellulose is generally dissolved by autolysis. Due to the existence of the "core-wrapping" problem, the uniformity of the product is affected, and the stability of the product is affected to a certain extent. On the other hand, it also creates some shackles on the production efficiency of some industries. For example, in the battery industry, with the rise of mobile phones and electric vehicles, the industry's demand for batteries has huge potential. Therefore, in mass production, there are clear speed requirements for each manufacturing step, and the "core-wrapping" problem is a shackle factor that must be considered in the battery production process.

[0005] For the "core-wrapping" problem, the main solution at present is to use some aldehyde products, such as glyoxal, to undergo an aldol condensation reaction with the hydroxyl groups on the surface of the product at a certain temperature, shielding the hydrophilic group hydroxyl groups on the surface of the powder, allowing the product to fully disperse after entering the water body and then slowly penetrate into the water and disperse, so as to solve the "core-wrapping" problem.

[0006] For example, in the invention patent with patent number 201510152478.0, a method for preparing instant sodium carboxymethyl cellulose is disclosed, wherein sodium carboxymethyl cellulose is prepared by alkalizing, etherifying and washing cellulose, and then glyoxal is added by spraying, and instant sodium carboxymethyl cellulose is prepared by drying and crushing. The above method has the following problems: the instant sodium carboxymethyl cellulose prepared by the aldol condensation reaction with glyoxal, glyoxal will fall off again and enter the water after encountering water, resulting in the presence of active groups such as glyoxal in the water body, and these residual active small molecules may react chemically with other substances in the later stage, posing a safety hazard to the final product quality. In addition, glyoxal is a toxic substance and is harmful to the human body. The instant sodium carboxymethyl cellulose prepared by this method can only be applied to a class of industrial fields that are not directly contacted by the human body, which limits the scope of application of the instant sodium carboxymethyl cellulose.

[0007] Another example is in the patent of invention of application number 200910200292.2, discloses a kind of preparation method of instant carboxymethyl cellulose, cellulose is prepared into sodium carboxymethyl cellulose by kneading method (alkalization, etherification), then neutralized, washed, dried, cross-linking agent (glyoxal, citric acid, alcohol solution) is added in the drying process, finally prepare instant sodium carboxymethyl cellulose. In the above method, glyoxal is used as the quick dissolving agent of sodium carboxymethyl cellulose, and there is toxicity problem when practical application. Simultaneously because of the crosslinking of glyoxal, the rise of molecular weight is caused, the viscosity of sodium carboxymethyl cellulose will be greatly improved, and the application of this sodium carboxymethyl cellulose in some fields is also limited.

[0008] The disclosure of the above background technology content is only used to assist in understanding the inventive concept and technical solution of the present invention. It does not necessarily belong to the prior art of this patent application. In the absence of clear evidence that the above content has been disclosed before the filing date of this patent application, the above background technology should not be used to evaluate the novelty and creativity of the present application. Summary of the invention

[0009] In view of this, in order to overcome the defects of the prior art, the present invention provides an improved instant sodium carboxymethyl cellulose, which can achieve rapid dissolution of sodium carboxymethyl cellulose, and the process and product are safe and non-toxic.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] A method for preparing sodium carboxymethyl cellulose comprises the following steps:

[0012] Add acetic acid and sodium acetate to the ethanol aqueous solution, dissolve and mix evenly to form a buffer solution;

[0013] Spraying the buffer solution onto the surface of sodium carboxymethyl cellulose powder and heating the powder to obtain sodium carboxymethyl cellulose with acidified surface;

[0014] The surface-acidified sodium carboxymethyl cellulose is added to an ethanol aqueous solution, and calcium carbonate powder is added, and the mixture is reacted at 10-40° C. for 1-3 hours to obtain a sodium carboxymethyl cellulose suspension with calcified powder surface.

[0015] According to some preferred implementation aspects of the present invention, the post-treatment step is included: centrifuging the sodium carboxymethyl cellulose suspension with calcified surface of the powder, removing the upper mother liquor, washing the lower precipitate with ethanol aqueous solution for multiple times, and drying the washed product to obtain the dried sodium carboxymethyl cellulose with calcified surface.

[0016] According to some preferred embodiments of the present invention, the powder particle size of the sodium carboxymethyl cellulose is 0.1-0.2 mm, preferably 0.106-0.18 mm, corresponding to a sieve of 80-150 mesh.

[0017] According to some preferred embodiments of the present invention, the mass ratio of acetic acid to sodium acetate in the buffer is 0.5-0.8:1.

[0018] According to some preferred embodiments of the present invention, the pH value of the buffer solution is 4.0-5.5.

[0019] According to some preferred implementation aspects of the present invention, the mass ratio of acetic acid to sodium carboxymethyl cellulose powder is 1:35-55.

[0020] According to some preferred embodiments of the present invention, the heating is maintained at 35-45° C. for 10-180 min.

[0021] According to some preferred implementation aspects of the present invention, the calcium carbonate is nano calcium carbonate, and the particle size of the nano calcium carbonate powder is 25 to 100 nm.

[0022] According to some preferred embodiments of the present invention, the mass ratio of the added amount of the calcium carbonate powder to the sodium carboxymethyl cellulose is 1-4:100.

[0023] According to some preferred embodiments of the present invention, the volume concentration of ethanol in the ethanol aqueous solution used in the buffer solution and / or the ethanol aqueous solution used in the washing is 60-95%.

[0024] According to some preferred embodiments of the present invention, the drying temperature is 105-120° C., and the drying time is 30-120 min.

[0025] In some embodiments of the present invention, the preparation method of instant sodium carboxymethyl cellulose specifically comprises the following steps:

[0026] (1) Preparation of buffer solution: Add acetic acid and sodium acetate into an ethanol aqueous solution, dissolve and mix well to prepare a buffer solution for later use.

[0027] (2) Surface acidification: The above buffer solution is evenly sprayed on the surface of the sodium carboxymethyl cellulose powder, and then baked in an oven at 35-45° C. for 10-180 min to obtain sodium carboxymethyl cellulose with acidified powder surface.

[0028] (3) Surface calcification: The surface-acidified sodium carboxymethyl cellulose is added to an ethanol aqueous solution and nano-calcium carbonate powder is added, and the mixture is reacted at 10-40° C. for 1-3 hours to obtain a sodium carboxymethyl cellulose suspension with calcified powder surface.

[0029] (4) Centrifugal separation: The sodium carboxymethyl cellulose suspension calcified on the surface of the powder is centrifuged to remove the upper mother liquor and wash the lower precipitate with ethanol aqueous solution for multiple times.

[0030] (5) Drying: Dry the washed product to obtain a finished product.

[0031] The centrifugal separation in step (4) and the drying in step (5) are post-processing steps. In some cases, the sodium carboxymethyl cellulose suspension with calcified powder surface obtained after the surface calcification in step (3) can be directly used in the next process.

[0032] The present invention also provides sodium carboxymethyl cellulose prepared according to the preparation method of sodium carboxymethyl cellulose.

[0033] The present invention also provides an application of the sodium carboxymethyl cellulose as described above in additives or auxiliary agents, such as food additives, cosmetics or coating auxiliary agents, battery electrode materials, etc.

[0034] The basic principle of the present invention is: the present invention first performs surface acidification and then performs surface calcification on sodium carboxymethyl cellulose powder to prepare instant sodium carboxymethyl cellulose. The present invention utilizes the characteristic that the surface calcium carboxymethyl cellulose can absorb water but cannot quickly absorb water to form a water ring after entering the water body, so that a complete water ring cannot be formed around this type of sodium carboxymethyl cellulose powder mass, and the water in the water body can quickly enter the interior of the sodium carboxymethyl cellulose powder through the disintegration gap, thereby achieving the purpose of rapid dissolution. The surface calcified sodium carboxymethyl cellulose utilizes calcium ions to combine with carboxylic acids to reduce the content of carboxylic acid anions, thereby reducing the problem of carboxymethyl cellulose anions absorbing water to form a "core", and at the same time, part of the calcium carbonate remaining between the sodium carboxymethyl cellulose powder can play the role of a disintegrant, prompting the sodium carboxymethyl cellulose powder to quickly disintegrate to form a uniform dispersion system, and the combination of the two aspects enables the sodium carboxymethyl cellulose to dissolve quickly and improve production efficiency. The small amount of calcified sodium carboxymethyl cellulose on the surface and the small amount of calcium carbonate powder between the particles will not cause changes in the performance of the internal sodium carboxymethyl cellulose and will not hinder the application performance of the sodium carboxymethyl cellulose. By spraying acidification with the prepared buffer, the pH value can be stabilized within a certain value, so that the acidification reaction only stays on the surface. Even if there is an excess of buffer on the surface of some particles, it will not further acidify the inside of the particles, causing excessive acidification, avoiding the increase of cellulose hydrogen and the decrease of the viscosity of the aqueous solution; at the same time, calcium carbonate is used to prepare the surface calcified sodium carboxymethyl cellulose. Since this product does not introduce toxic substances during the preparation process and is non-toxic itself, it can solve the toxicity problems caused by other processes such as: instant sodium carboxymethyl cellulose prepared by glyoxal cross-linking agent.

[0035] By adopting the above technical scheme, compared with the prior art, the advantages of the present invention are as follows: the sodium carboxymethyl cellulose of the present invention adopts calcium carbonate to carry out surface modification of the sodium carboxymethyl cellulose, the process flow is simple and the cost is low, and at the same time, the "core wrapping" problem during dissolution and the product quality and toxicity problems that may exist in the later stage are solved, thereby expanding the application field of the instant sodium carboxymethyl cellulose; the use of the matching buffer solution can avoid the product quality problems caused by excessive acidification. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0037] Figure 1 The solubility comparison results of the instant sodium carboxymethyl cellulose prepared in the examples of the present invention and the sodium carboxymethyl cellulose in the comparative example are shown. DETAILED DESCRIPTION

[0038] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0039] In order to solve the problems of "core wrapping" and "unsafety" at the same time, the preparation method of the instant sodium carboxymethyl cellulose of the present invention adopts a buffer solution for surface acidification and then adopts calcium carbonate to modify the surface of the sodium carboxymethyl cellulose, so as to reduce the risk that the currently available instant sodium carboxymethyl cellulose may have potential safety hazards to later products, and improve the application scope of the instant sodium cellulose.

[0040] The instant type in the present invention is defined as: when poured into an aqueous solution stirred at room temperature, no obvious clumping phenomenon occurs, and the phenomenon is first dispersed and then dissolved; it only disperses within 2 minutes after entering the water without releasing viscosity, and then the surface disintegrates and absorbs water to quickly release viscosity, the time for the viscosity to reach the maximum value does not exceed 20 minutes, and the final viscosity of the 1% aqueous solution deviates from the viscosity value of conventional dissolution by no more than 5%.

[0041] The preparation method of instant sodium carboxymethyl cellulose in this embodiment uses sodium carboxymethyl cellulose powder as raw material, and comprises the following steps:

[0042] (1) Buffer preparation

[0043] Add acetic acid and sodium acetate to the ethanol aqueous solution, dissolve and mix evenly to prepare a buffer solution with a pH value of 4.0-5.5 for later use.

[0044] The volume concentration of ethanol in the ethanol aqueous solution used is 60-95%. The mass ratio of acetic acid to sodium acetate in the buffer solution is 0.5-0.8:1.

[0045] (2) Surface acidification

[0046] The above buffer solution is evenly sprayed on the surface of sodium carboxymethyl cellulose powder (powder particle size is between 80-150 mesh screen), and then baked in an oven at 35-45°C for 10-180 minutes to obtain sodium carboxymethyl cellulose with acidified powder surface. The mass ratio of acetic acid to sodium carboxymethyl cellulose powder in the buffer solution is 1:35-55.

[0047] By spraying acidification with the prepared buffer, the pH value can be stabilized within a certain value, so that the acidification reaction only stays on the surface. Even if there is an excess of buffer on the surface of some particles, it will not cause excessive acidification. At the same time, even if the surface of the particles is not completely acidified to form a partial water layer, water can still enter the cellulose interior through the other disintegration layer on the surface of the particles (i.e. the calcified part) to dissolve.

[0048] During the process of spraying the buffer solution, the nozzle is above the particles, and the sodium carboxymethyl cellulose particles are allowed to roll under the nozzle. The sodium carboxymethyl cellulose particles are then collected and fully stirred to fully disperse the liquid adsorbed on the surface of the particles. The wet solid is then moved into an oven for baking to promote the acidification reaction.

[0049] (3) Surface calcification

[0050] The surface-acidified sodium carboxymethyl cellulose is added to an ethanol aqueous solution, and nano-calcium carbonate powder is added, and the mixture is reacted at 10-40° C. for 1-3 hours to obtain a sodium carboxymethyl cellulose suspension with calcified powder surface.

[0051] The particle size of the nano calcium carbonate powder is 25-100 nm. The mass ratio of the added amount of calcium carbonate powder to sodium carboxymethyl cellulose is 1-4:100. The residual calcium carbonate after the reaction is subsequently located between adjacent sodium carboxymethyl cellulose particles, which can play the role of a disintegrant, further promoting the rapid disintegration of the sodium carboxymethyl cellulose powder to form a uniform dispersion system.

[0052] (4) Centrifugal separation

[0053] The sodium carboxymethylcellulose suspension with calcified powder surface is centrifuged to remove the upper mother liquor, and the lower precipitate is washed three times with an ethanol aqueous solution, wherein the volume concentration of ethanol in the ethanol aqueous solution used for washing is 60-95%.

[0054] (5) Drying

[0055] The washed product is dried to obtain a finished product at a drying temperature of 105-120°C and a drying time of 30-120 minutes.

[0056] The centrifugal separation in step (4) and the drying in step (5) are post-processing steps. In some cases, the sodium carboxymethyl cellulose suspension with calcified powder surface obtained after the surface calcification in step (3) can be directly used in the next process.

[0057] Example 1

[0058] The preparation method of instant sodium carboxymethyl cellulose in this embodiment uses sodium carboxymethyl cellulose powder as raw material, and comprises the following steps:

[0059] Add 76 ml of glacial acetic acid, 100 g of sodium acetate, and 200 g of 70% ethanol aqueous solution to a beaker to prepare a buffer solution. Take 50 g of the above buffer solution and spray it evenly on 400 g of CMC powder, and move it into a 40°C oven for baking for 60 min. Add the above baked powder to 600 g of 90% ethanol aqueous solution, and add 8.5 g of nano calcium carbonate solid powder to react at 30°C for 60 min, then centrifuge and wash it 3 times with 75% ethanol aqueous solution, and dry it to obtain instant sodium carboxymethyl cellulose.

[0060] Example 2

[0061] The preparation method of instant sodium carboxymethyl cellulose in this embodiment uses sodium carboxymethyl cellulose powder as raw material, and comprises the following steps:

[0062] Add 76 ml of glacial acetic acid, 120 g of sodium acetate, and 200 g of 70% ethanol aqueous solution to a beaker to prepare a buffer solution. Take 43.8 g of the above buffer solution and spray it evenly on 400 g of CMC powder, and move it into a 40°C oven for baking for 90 min. Add the above baked powder to 600 g of 90% ethanol aqueous solution, and add 7.5 g of nano calcium carbonate solid powder to react at 30°C for 1 hour, then centrifuge and wash it with 75% ethanol aqueous solution for 3 times, and dry it to obtain instant sodium carboxymethyl cellulose.

[0063] Example 3

[0064] The preparation method of instant sodium carboxymethyl cellulose in this embodiment uses sodium carboxymethyl cellulose powder as raw material, and comprises the following steps:

[0065] Add 76 ml of glacial acetic acid, 120 g of sodium acetate, and 200 g of 70% ethanol aqueous solution to a beaker to prepare a buffer solution. Take 37.5 g of the above buffer solution and spray it evenly on 400 g of CMC powder, and move it into a 40°C oven for baking for 90 min. Add the above baked powder to 600 g of 90% ethanol aqueous solution, add 7.5 g of nano calcium carbonate solid powder, and react at 40°C for 2 h, then centrifuge and wash it 3 times with 75% ethanol aqueous solution, and dry it to obtain instant sodium carboxymethyl cellulose.

[0066] Example 4

[0067] The preparation method of instant sodium carboxymethyl cellulose in this embodiment uses sodium carboxymethyl cellulose powder as raw material, and comprises the following steps:

[0068] Add 76ml of glacial acetic acid, 150g of sodium acetate, and 200g of 90% ethanol aqueous solution in a beaker to prepare a buffer solution. Take 50g of the above buffer solution and spray it evenly on 400g of CMC powder, and move it into a 40℃ oven for baking for 180min. Add the above baked powder to 600g of 90% ethanol aqueous solution, add 8.5g of nano calcium carbonate solid powder, and react at 40℃ for 2h, then centrifuge and wash 3 times with 75% ethanol aqueous solution, and dry to obtain instant sodium carboxymethyl cellulose.

[0069] Comparative Example 1

[0070] The sodium carboxymethyl cellulose in this comparative example is the raw material of the embodiment, that is, the sodium carboxymethyl cellulose powder without surface modification, and its particle size distribution is consistent with the raw material sodium carboxymethyl cellulose in the embodiment, which is 0.106-0.18mm (i.e., particles between 80-150 meshes).

[0071] Comparative Example 2

[0072] The difference between this comparative example and Example 1 is that in this comparative example, no buffer solution is used to acidify the sodium carboxymethyl cellulose.

[0073] The method for preparing instant sodium carboxymethyl cellulose in this comparative example uses sodium carboxymethyl cellulose powder as a raw material, and comprises the following steps:

[0074] Add 76ml of glacial acetic acid and 200g of 70% ethanol aqueous solution into a beaker, mix well and set aside. Take 35g of the above solution and spray it evenly on 400g CMC powder, and move it into a 40℃ oven for baking for 60min. Add the above baked powder into 600g of 90% ethanol aqueous solution, and add 8.5g of nano calcium carbonate solid powder to react at 30℃ for 60min, then centrifuge and wash it 3 times with 75% ethanol aqueous solution, and dry it to obtain sodium carboxymethyl cellulose.

[0075] Tests and Results

[0076] The viscosity changes (constant temperature 25° C.) of the instant sodium carboxymethyl cellulose prepared in the example, the untreated sodium carboxymethyl cellulose (Comparative Example 1) and the comparative example 2 during dissolution were tested, and the experimental method was as follows:

[0077] 1. Add 198 g of deionized water to a 250 mL beaker and place in a magnetic stirrer.

[0078] 2. Place the beaker on the magnetic stirrer and adjust the height of the viscometer so that the rotor scale of the viscometer just falls on the horizontal plane.

[0079] 3. Program the viscometer to control it to read a viscosity value every 1 minute.

[0080] 4. Turn on magnetic stirring and set the speed to 100 rpm.

[0081] 5. Pour 2g CMC powder within 1 minute, and immediately turn on the viscometer for automatic testing.

[0082] 6. Stop the test after 60 minutes and observe the viscosity changes.

[0083] The experimental results are as follows Figure 1 shown.

[0084] from Figure 1 It can be seen that the four samples of the embodiment have good instant dissolution effect. After 3-8 minutes of disintegration time, the instant CMC dissolves rapidly, causing a rapid increase in viscosity. Within 10-20 minutes, the viscosity reaches equilibrium, indicating that the dissolution time is only 10-20 minutes, which is an instant CMC. As for the CMC of comparative example 1, after adding water, the viscosity first rises slowly and then gradually accelerates, indicating that water is slowly absorbed and dissolved by the CMC powder, that is, a water layer is formed outside the CMC powder, resulting in slow dissolution of the internal CMC. In the later stage, it is necessary to stir all the time to promote the uniform dissolution of the internal CMC. As time goes on, the viscosity keeps rising, and equilibrium has not been reached in 50 minutes, and the dissolution time is more than 50 minutes. The CMC of comparative example 2 has a good instant dissolution effect as in the embodiment, but the viscosity of its aqueous solution decreases significantly. The reason is that the acidification performance of the unused buffer is stronger, and the acid can easily penetrate into the interior of the sodium carboxymethyl cellulose for acidification. The over-acidified part inside cannot contact with calcium carbonate and cannot be calcified. Finally, part of the CMC exists in the form of carboxymethyl cellulose hydrogen (insoluble in water and does not produce viscosity), which increases the insoluble impurities in the water, reduces the viscosity of the aqueous solution, and affects the performance of the product.

[0085] In Example 3, due to less calcification, the surface calcium carboxymethyl cellulose required less time to disintegrate, and the overall dissolution time was shorter. In Example 4, the reaction time was increased, the calcification was relatively more, and the surface calcium carboxymethyl cellulose required a longer time to disintegrate, which increased the dissolution time overall.

[0086] The preparation method of the instant sodium carboxymethyl cellulose of the present invention comprises the following steps: preparing acetic acid and sodium acetate buffer, and spraying the buffer on the surface of sodium carboxymethyl cellulose powder; preparing the surface acidified sodium carboxymethyl cellulose by low temperature baking; then adding the baked solid and calcium carbonate solid into ethanol aqueous solution to prepare the surface calcified sodium carboxymethyl cellulose; and then washing, filtering and drying to prepare the product. The instant sodium carboxymethyl cellulose prepared by the method not only does not leave any active substance in the water body, but also has a simple process and is easy to realize industrial production. In addition, the product prepared by this process is safe and non-toxic and can be applied to food and other fields; the acidification by the buffer ensures the product quality.

[0087] The equipment and raw materials used in the above-mentioned embodiments can be purchased from the market or are commonly used in this field. The methods in the above-mentioned embodiments, if not otherwise specified, are conventional methods in this field. The raw materials not specifically specified in the embodiments are all obtained commercially. The operation without special mention of temperature is carried out at room temperature. The operating methods and conditions not specifically specified can adopt the known or conventional means and conditions in this field. The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0088] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A sodium carboxymethyl cellulose, characterized in that The sodium carboxymethyl cellulose powder is surface acidified by using a buffer solution, and then the surface of the sodium carboxymethyl cellulose is calcified by using calcium carbonate. The buffer solution is prepared by adding acetic acid and sodium acetate to an ethanol aqueous solution, dissolving and mixing them uniformly to form a buffer solution. In the prepared sodium carboxymethyl cellulose, the residual part of calcium carbonate is located between adjacent sodium carboxymethyl cellulose particles, playing the role of a disintegrant, further promoting the rapid disintegration of sodium carboxymethyl cellulose powder to form a uniform dispersion system.

2. The sodium carboxymethyl cellulose according to claim 1, characterized in that The sodium carboxymethyl cellulose only disperses without releasing viscosity within 2 minutes after entering water, and then the surface disintegrates and absorbs water to release viscosity.

3. The sodium carboxymethyl cellulose according to claim 1, characterized in that The time for the sodium carboxymethyl cellulose viscosity to reach the maximum value does not exceed 20 minutes, and the final viscosity of the 1% aqueous solution deviates from the viscosity value of conventional solution by no more than 5%.

4. The sodium carboxymethyl cellulose according to claim 1, characterized in that The surface acidification is to spray the buffer solution for acidification. During the spraying of the buffer solution, the nozzle is above the particles, and the sodium carboxymethyl cellulose particles are allowed to roll under the nozzle. The sodium carboxymethyl cellulose particles are then collected and fully stirred to fully disperse the liquid adsorbed on the surface of the particles. The wet solid is then moved into an oven for baking to promote the acidification reaction.

5. The sodium carboxymethyl cellulose according to claim 1, characterized in that The particle size of the sodium carboxymethyl cellulose powder is 0.1-0.2 mm.

6. The sodium carboxymethyl cellulose according to claim 1, characterized in that The mass ratio of acetic acid to sodium acetate in the buffer solution is 0.5-0.8:

1.

7. The sodium carboxymethyl cellulose according to claim 1, characterized in that The pH value of the buffer solution is 4.0-5.

5.

8. The sodium carboxymethyl cellulose according to claim 1, characterized in that The mass ratio of the acetic acid to the sodium carboxymethyl cellulose powder is 1:35-55.

9. The sodium carboxymethyl cellulose according to claim 1, characterized in that The calcium carbonate is nano calcium carbonate, and the particle size of the nano calcium carbonate powder is 25-100 nm.

10. The sodium carboxymethyl cellulose according to claim 1, characterized in that The mass ratio of the added amount of the calcium carbonate powder to the sodium carboxymethyl cellulose is 1-4:

100.

11. The sodium carboxymethyl cellulose according to any one of claims 1 to 10, characterized in that The sodium carboxymethyl cellulose is prepared by the following steps: (1) Preparation of buffer solution: Add acetic acid and sodium acetate into an ethanol aqueous solution, dissolve and mix evenly to prepare a buffer solution for later use; (2) Surface acidification: spraying the buffer solution uniformly on the surface of the sodium carboxymethyl cellulose powder and heating to obtain the sodium carboxymethyl cellulose with acidified powder surface; (3) Surface calcification: The surface-acidified sodium carboxymethyl cellulose is added to an ethanol aqueous solution and nano-calcium carbonate powder is added to obtain a sodium carboxymethyl cellulose suspension with calcified powder surface after reaction.

12. The sodium carboxymethyl cellulose according to claim 11, characterized in that The reaction is carried out at 10-40°C for 1-3 hours.

13. The sodium carboxymethyl cellulose according to claim 11, characterized in that The heating is maintained at 35-45°C for 10-180 minutes.

14. The sodium carboxymethyl cellulose according to claim 11, characterized in that The steps include: (4) centrifugal separation: centrifuging the sodium carboxymethyl cellulose suspension calcified on the surface of the powder, removing the upper mother liquor, and washing the lower precipitate with ethanol aqueous solution for multiple times; (5) Drying: Drying the washed product to obtain dried surface calcified sodium carboxymethyl cellulose.

15. Use of the sodium carboxymethyl cellulose according to any one of claims 1 to 14 in additives or auxiliary agents, wherein the additive is a food additive, and the auxiliary agent is a cosmetic auxiliary agent or a coating auxiliary agent.

Citation Information

Cited By

  • Carboxymethylcellulose sodium sustained-release microspheres and a preparation method thereof

    CN122786288A