Chiral thermally activated delayed fluorescent polymer and application thereof
By synthesizing new axial chiral TADF polymers, using materials such as binaphthalene derivatives and acridines, the polymer structure is optimized, and the problems of high manufacturing cost and racemic risk of white circular polarization WOLED devices are solved, achieving efficient electrogenesis Circular polarization single white light emission and high external quantum efficiency.
Patent Information
- Application Number
- CN202410944189.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Existing white circularly polarized organic light emitting diode (WOLED) devices rely on a two-layer structure, are costly and have racemic risks, making it difficult to achieve efficient electrocyclic polarized single white light emission.
Binaphthalene derivatives are used as chiral source, benzophenone is an electron acceptor, and acridine is an electron donor. By adjusting the proportion of TADF units, a new axial chiral TADF polymer is synthesized and suspended on the side chain of the polystyrene framework. , optimize the polymer structure to achieve circularly polarized luminescence, and use a non-conjugated polymerization strategy to reduce energy loss as a light-emitting layer material for white circularly polarized organic light-emitting diodes.
A white circularly polarized organic light-emitting diode with high external quantum efficiency (10.8-15.1%) is achieved, reducing device driving voltage, avoiding racemization risks, and improving the luminous efficiency and stability of the material.
Smart Images

Figure CN118909173A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic electroluminescent materials, and specifically discloses a class of chiral thermally activated delayed fluorescent polymers and applications thereof. Background Art
[0002] In recent years, circularly polarized luminescent materials have shown broad application prospects in the fields of optical data storage, chiral sensing, bio-responsive imaging, asymmetric synthesis, and chiral materials. In addition to the application of circularly polarized photoluminescence, the development of circularly polarized electroluminescence (CPEL) has also attracted widespread attention and is considered to be more valuable in optoelectronic technology. Since Meijer et al. first reported circularly polarized polymer light-emitting diodes (CP-PLEDs) in 1997, CPELs of CP-PLEDs have developed rapidly. However, due to the theoretical internal quantum efficiency (IQE) of 25%, conventional fluorescent polymer materials cannot achieve satisfactory performance in CP-PLED devices. In order to achieve more efficient CPELs, chiral phosphorescent complexes with a theoretical IQE of 100% are used as luminescent materials for the corresponding devices. However, phosphorescent materials still face problems such as high cost, environmental issues, and instability of coordination bonds.
[0003] As the third generation of light-emitting materials, thermally activated delayed fluorescence (TADF) materials with pure organic molecular structures can achieve the same 100% theoretical IQE as phosphorescent materials and are considered to be promising pure organic materials for manufacturing organic light-emitting diodes (OLEDs). Unlike traditional fluorescent emission materials, TADF materials always have a sufficiently small singlet-triplet energy gap (ΔE) due to the sufficient separation of the distribution of the highest occupied molecular orbitals (HOMOs) and the lowest unoccupied molecular orbitals (LUMOs). ST ), which is less than 0.3 eV. Therefore, triplet excitons can be fully utilized through the reverse intersystem crossing (RISC) process without the need for additional energy supply, thus improving the exciton utilization rate.
[0004] As a new type of solid-state light source, white organic light-emitting diode (WOLED) has shown broad application prospects in the field of lighting. WOLED with high external quantum efficiency (EQE) and high color rendering index (CRI) can bring advantages such as good color rendering effect and long service life to white light sources, so it has become the research focus of academia and industry.
[0005] In order to achieve efficient white light emission, it is necessary to simultaneously include a certain proportion of the three primary colors (blue, green, and red) or two complementary colors (blue with orange or yellow) in the emission layer. In this regard, various strategies have been used to obtain white light emission, such as physically mixing monochromatic luminescent materials into host polymer materials, or chemically tethering luminescent materials to polymer chains. Compared with chiral small molecules, chiral polymers are easier to achieve single white light emission by controlling the proportion of different emission colors during polymerization. In 2022, Cheng Yixiang's research group designed a class of chiral white light polymers S- / R-WP1 and S- / R-WP2 by copolymerizing binaphthyl derivative units with three blue, green, and red luminescent units. The standard white CP-OLED based on S- / R-WP2 has a CRI of up to 95 at the International Commission on Illumination (CIE) coordinates (0.33, 0.34). In the wavelength range of 425 to 760 nm, the maximum brightness (L max ) is about 3000cd m -2 , electroluminescence asymmetry factor (g EL ) is 10 -3 , but its EQE max Only 0.54%.
[0006] Exciplex is a kind of intermolecular charge transfer excited state luminescence composed of electron donor and electron acceptor. Compared with single-molecule luminescent materials of donor and acceptor, exciplex has larger Stokes shift and wider emission peak, which is conducive to the construction of white light OLEDs; at the same time, the new exciplex system with TADF characteristics can achieve high exciton utilization through effective upconversion of triplet excitons, improve device efficiency, and has a lower energy gap, thereby reducing the device driving voltage. Therefore, combining the advantages of exciplex in achieving white light emission and high exciton utilization, it is of great significance to build efficient white circularly polarized organic light-emitting diodes based on it.
[0007] Most of the white circularly polarized organic light-emitting diodes reported so far rely on double-layer devices. As an alternative approach, there is a growing demand for placing different chiral luminescent materials in a single luminescent layer to realize CP-WOLED. Recently, Chen Chuanfeng's research group realized CP-WOLED based on the strategy of integrating conformational isomerization donors and chiral acceptors in a single molecule. Unfortunately, this CP-WOLED needs to be realized through a vacuum evaporation process, which has harsh conditions, high manufacturing costs, and a potential risk of racemization. Therefore, it is of great significance to continue to propose new construction strategies to achieve efficient electro-induced circularly polarized single white light emission. Summary of the invention
[0008] In order to further reduce ΔE STIn order to obtain more efficient TADF materials. The present invention uses binaphthyl derivatives as chiral sources, benzophenone as electron acceptors, and acridine as electron donors. The binaphthyl chiral source is directly introduced into the TADF unit and suspended on the side chain of the polystyrene skeleton. A series of chiral green light TADF polymers (R)-E-0.02 / (S)-E-0.02 are designed and synthesized by adjusting the ratio of TADF units during polymerization.
[0009] (R)-E-0.05 / (S)-E-0.05 and (R)-E-0.1 / (S)-E-0.1. By optimizing the ratio of chiral TADF units in the polymer, the polymer (R)-E-0.1 / (S)-E-0.1 can detect obvious circularly polarized luminescence signals in both the ground state and the excited state, and the binaphthyl chiral source can effectively induce the circularly polarized luminescence of the polymer. In the scheme, benzophenone is an electron acceptor and acridine is an electron donor. The combination of the two is conducive to the separation of the highest occupied orbital (HOMO) and the lowest occupied orbital (LUMO) of the TADF unit in the polymer, which is beneficial to reduce the energy gap difference between the single triplet state and improve the luminescence efficiency of the material.
[0010] The present invention first synthesizes a new type of axial chiral TADF polymer material with binaphthyl derivatives as chiral sources, benzophenone as electron acceptor, and acridine as electron donor. The material has the following structure:
[0011]
[0012] The present invention also provides a method for preparing a chiral thermally activated delayed fluorescence polymer, using a binaphthyl derivative as a chiral source, benzophenone as an electron acceptor, and acridine as an electron donor, and directly introducing the binaphthyl chiral source into the TADF unit, suspending it on the side chain of the polystyrene skeleton, and synthesizing a series of chiral green light thermally activated delayed fluorescence polymers by adjusting the ratio of the TADF unit during polymerization using a non-conjugated polymerization strategy, optimizing the ratio of the chiral TADF monomer during polymerization, and systematically studying the structure-activity relationship of the material.
[0013] The binaphthyl derivative is (R / S)-binaphthol, which has the advantages of cross-stable spatial configuration, strong chiral induction ability, and low price.
[0014] The proportion of chiral TADF units is 2%-10%.
[0015] The present invention also provides an application of a novel axially chiral TADF polymer material as a light-emitting layer material for a white circularly polarized organic light-emitting diode. By using a solution processing method, a chiral thermally activated delayed fluorescence polymer material is used as a light-emitting layer or a light-emitting layer dopant to prepare the light-emitting layer of a white circularly polarized organic light-emitting diode, thereby obtaining a white circularly polarized organic light-emitting device with excellent light-emitting performance.
[0016] The mass percentage of the chiral luminescent material as a dopant in the luminescent layer is 50-90wt%.
[0017] The external quantum efficiency of a white circularly polarized organic light-emitting diode prepared by using a chiral thermally activated delayed fluorescent polymer material as a light-emitting layer or a light-emitting layer dopant is 10.8-15.1%.
[0018] The technical advantages of the present invention are:
[0019] 1. Using benzophenone as the electron acceptor and acridine as the electron donor, the combination of the two is conducive to the separation of the highest occupied orbital (HOMO) and the lowest occupied orbital (LUMO) of the polymer, which is conducive to reducing ΔE ST , it is easy to obtain TADF materials and improve the luminescence efficiency of the materials; the thermally activated delayed fluorescent material is non-conjugated with the chiral source of binaphthyl, and the non-conjugated polymer main chain has high triplet energy, which can reduce unnecessary energy loss from the TADF unit to the polymer main chain. Based on this polymerization method, a series of new axial chiral TADF polymer luminescent materials are constructed; by optimizing the proportion of chiral TADF units in the polymer, it is given enhanced circularly polarized luminescence properties while maintaining the photophysical properties of the TADF unit;
[0020] 2. Based on the synthesized chiral TADF polymer as the acceptor and the commercial achiral TAPC as the donor, the light-emitting layer dopant was constructed to obtain a high-efficiency solution-processed electroexcimer white light device. BRIEF DESCRIPTION OF THE DRAWINGS
[0021]
Figure 1
[0022]
Figure 2
[0023]
Figure 3
[0024]
Figure 4
[0025]
Figure 5
[0026]
Figure 6
[0027]
Figure 7
[0028]
Figure 8
[0029]
Fig. 9
[0030]
Fig.10
[0031]
Fig.11
[0032]
Fig.12
[0033]
Fig.13
[0034]
Fig.14
[0035]
Fig.15
[0036]
Fig.16
[0037]
Fig.17
[0038]
Fig.18
[0039]
Fig.19
[0040]
Fig. 20
[0041]
Fig.21
[0042]
Fig. 22
[0043] The following specific implementation cases are intended to further illustrate the present invention, but these specific implementation cases do not limit the protection scope of the present invention in any way.
[0044] Example 1 Chiral TADF Polymer Synthesis:
[0045]
[0046] Synthesis of compound 1
[0047] The following raw materials were added to a 100 mL single-necked flask in sequence: p-bromobenzophenone (3.0 g, 11.5 mmol), 9,10-dihydro-9,9-dimethylacridine (3.6 g, 17.3 mmol), sodium tert-butoxide (3.3 g, 34.5 mmol), tri-tert-butylphosphine tetrafluoroborate (334.0 mg, 1.2 mmol), palladium acetate (232.0 mg, 1.0 mmol) and 50.0 mL toluene, and N2 was passed through the reaction mixture, and the mixture was reacted at 90°C for 18 h. The reaction mixture was cooled to room temperature, the solvent was removed by rotary evaporation, and then the mixture was extracted three times with DCM, washed three times with water, dried over anhydrous magnesium sulfate, filtered and the filtrate was collected, the solvent was dried again, and PE and DCM were used as eluents (volume ratio 4:1), and 4.4 g of yellow solid was obtained by column chromatography, with a yield of 98%. 1 H NMR (400MHz, CD2Cl2) δ (ppm) 8.00-7.96 (m, 2H), 7.83-7.80 (m, 2H), 7.57 (ddd, J = 6.8, 4.0, 1.3Hz, 1H), 7.48 (tt ,J=6.7,1.2Hz,2H),7.41(dd,J=6.3,4.4Hz,4H),6.94-6.84(m,4H),6.26(dd,J=8.0,1.4Hz,2H),1.60(s,6H). 13CNMR (101MHz, CDCl3) δ (ppm) 152.78, 151.72, 132.30, 131.65, 130.65, 130.14, 128. 27,127.05,126.22,125.86,125.04,121.86,83.98,25.23,24.67.TOF-MS(ESI)m / z calcd for C 28 H 23 NO:390.08;[M+H]+found:389.18.
[0048] Synthesis of compound 2
[0049] Compound 1 (850.0 mg, 2.2 mmol) and 30.0 mL of anhydrous chloroform were added to a 100 mL single-mouth bottle, and N-bromosuccinimide (971.0 mg, 5.5 mmol) dissolved in 20.0 mL of anhydrous chloroform was added dropwise at 0°C, and then reacted at room temperature in the dark for 12 h. After the reaction was completed, the solvent was dried, and the crude product was precipitated with DCM and MeOH solvents, and filtered to obtain 1.1 g of a yellow solid with a yield of 91%. 1 H NMR (400MHz, CDCl3) δ (ppm) 8.08 (d, J = 7.6Hz, 2H), 7.90 (d, J = 7.4Hz, 2H), 7.65 (t, J = 7.1Hz, 1H), 7. 58-7.50 (m, 4H), 7.43 (d, J=7.6Hz, 2H), 7.09 (d, J=8.6Hz, 2H), 6.18 (d, J=8.6Hz, 2H), 1.65 (s, 6H). 13 C NMR (101MHz, CDCl3) δ (ppm) 195.72, 144.30, 139.33, 137.73, 137.07, 132.97, 1 31.96, 130.89, 130.14, 129.45, 128.58, 128.27, 115.92, 113.85, 36.37, 30.92. TOF-MS(ESI)m / z calcd for C 28 H 21 Br2NO[M+H]+:546.01; found:548.11.
[0050] Synthesis of compound 3
[0051] In a 200mL single-mouth bottle, (R / S)-binaphthol (5.0g, 17.5mmol), 1,4-dibromo-2,3-difluorobenzene (5.2g, 19.2mmol), cesium carbonate (11.4g, 35.0mmol), and 100.0mL anhydrous DMF were added in sequence, and the mixture was heated to 120°C under nitrogen (N2) protection to react overnight. The reaction solution was cooled to room temperature, and the solvent was removed by rotary evaporation, and then extracted three times with dichloromethane (DCM), washed three times with water, dried over anhydrous magnesium sulfate, filtered and collected, and the solvent was dried again, and petroleum ether (PE) and DCM (volume ratio 7:1) were used as eluents. 4.3g of white solid was obtained by column chromatography, and the yield was 47%. 1 H NMR (400MHz, CDCl3) δ (ppm) 8.00 (d, J = 8.8Hz, 2H), 7.95 (d, J = 8.2Hz, 2H), 7.60-7.55 (m, 4H), 7.50 (t, J = 7.4Hz, 2H), 7.39 (t, J = 7.5Hz, 2H), 7.27 (s, 2H). 13 C NMR (101MHz, CDCl3) δ (ppm) 150.49, 147.73, 132.07, 132.03, 130.98, 128.65, 128.46, 126.94, 126.85, 125.79, 125.46, 121.20, 115.70.
[0052] Synthesis of compound 4
[0053] Phenylboric acid (117.6 mg, 0.96 mmol), compound 3 (1.0 g, 1.9 mmol), sodium carbonate (2.0 g, 19.3 mmol), tetrakistriphenylphosphine palladium (111.5 mg, 0.096 mmol), 30.0 mL tetrahydrofuran and 15.0 mL water were added to a 100 mL single-mouth bottle, and the mixture was heated to 80 ° C under nitrogen protection for 24 h. The reaction solution was cooled to room temperature, the solvent was removed by rotary evaporation, extracted three times with dichloromethane (DCM), washed three times with water, dried over anhydrous magnesium sulfate, filtered and collected The filtrate was dried again, and the solvent was dried again, and PE and DCM (volume ratio 8:1) were used as eluents. 305.0 mg of a white solid was obtained by column chromatography, and the yield was 31%. 1 H NMR (400MHz, CD2Cl2) δ (ppm) 7.99 (d, J = 8.8Hz, 1H), 7.95-7.91 (m, 1H), 7.83 (d, J = 8.2Hz, 1H), 7.77 (d, J=8.8Hz,1H),7.59(d,J=8.8Hz,1H),7.47-7.27(m,12H),7.02(d,J=8.4Hz,1H),6.84(d,J=8.8Hz,1H).13 C NMR (101MHz, CDCl3) δ (ppm) 150.93, 150.85, 147.24, 147.17, 136.84, 135.36, 132.04, 131.98, 131.90, 131.63, 130.66, 130.56, 129.69 ,128.42,128.29,128.17,127.99,127.60,126.83,126.73,126.63,126.16,125.73,125.48,125.42,125.37,121.53,120.94,115.25.
[0054] Synthesis of compound 5
[0055] Compound 4 (0.3 g, 0.58 mmol), bipyraclostrobin (177.4 mg, 0.698 mmol), potassium acetate (285.6 mg, 2.9 mmol), [1,1'-bis(diphenylphosphino)ferrocene] palladium dichloride (21.3 mg, 0.029 mmol), and 25.0 mL of analytically pure toluene solution were added to a 50 mL single-mouth bottle in sequence, and the mixture was heated to 110 ° C under N2 protection for 24 h. The reaction solution was cooled to room temperature, and toluene was removed by rotary evaporation, extracted three times with DCM, washed three times with water, dried over anhydrous magnesium sulfate, filtered and collected, and the solvent was dried again, and then directly used in the next step of reaction after vacuum drying.
[0056] Synthesis of compound 6
[0057] Compound 2 (250.0 mg, 0.5 mmol), compound 5 (183.0 mg, 0.2 mmol), sodium carbonate (484.0 mg, 4.6 mmol), tetrakistriphenylphosphine palladium (26.4 mg, 0.00002 mmol), 15.0 mL tetrahydrofuran and 7.5 mL water were added to a 50 mL single-mouth bottle in sequence, and the mixture was heated to 80 ° C under N2 protection for 24 h. The reaction solution was cooled to room temperature, the solvent was removed by rotary evaporation, extracted three times with DCM, washed three times with water, dried over anhydrous magnesium sulfate, filtered and the filtrate was collected, the solvent was dried again, and PE and DCM (volume ratio 4:1) were used as eluents. The yellow solid 73.0 mg was separated by column chromatography with a yield of 18%. 1H NMR (400MHz, CD2Cl2) δ (ppm) 7.95 (d, J = 8.4Hz, 2H), 7.85 (t, J = 9.0Hz, 3H), 7.80-7.77 (m, 3H) ,7.65(d,J=2.0Hz,1H),7.58-7.49(m,4H),7.47-7.38(m,8H),7.37-7.33(m,2H),7.28(dd,J =12.4,5.2Hz,3H),7.22-7.16(m,3H),7.08(d,J=8.8Hz,1H),7.02(dt,J=8.8,2.6Hz,1H),6. 93(d,J=8.8Hz,1H),6.27(d,J=8.6Hz,1H),6.15(d,J=8.8Hz,1H),1.66(s,3H),1.60(s,3H). 13 C NMR (101MHz, CDCl3) δ (ppm) 195.74, 151.45, 151.36, 146.98, 146.85, 144.57, 139.51, 139.28, 137.65, 137.46, 13 7.10,134.45,134.34,132.79,132.75,132.47,132.04,131.56,131.51,131.01,130.57,130.29,130.06,129.82, 129.49,129.21,128.46,128.35,128.32,128.29,128.09,127.27,126.75,126.70,126.44,126.39,125.78,125.7 5,125.41,125.20,125.16,125.11,121.30,115.80,113.87,113.46,36.35,31.42,31.22,26.89.TOF-MS(ESI)m / z calcd for C 60 H 40 BrNO3:901.22;[M+H]+found:902.33.
[0058] Synthesis of compound 7
[0059] Compound 6 (165.0 mg, 0.2 mmol), vinylboronic acid pinacol ester (42.0 mg, 0.3 mmol), sodium hydroxide (73.0 mg, 1.8 mmol), tetrakistriphenylphosphine palladium (11.0 mg, 0.009 mmol), 15.0 mL tetrahydrofuran and 7.5 mL water were added to a 50 mL single-mouth bottle in sequence, and the mixture was heated to 80 ° C for 24 h under N2 protection. The reaction solution was cooled to room temperature, the solvent was removed by rotary evaporation, extracted three times with DCM, washed three times with water, dried over anhydrous magnesium sulfate, filtered and the filtrate was collected, the solvent was dried again, and PE and DCM (volume ratio 3: 1) were used as eluents. The yellow solid 100.0 mg was separated by column chromatography with a yield of 65%. 1 HNMR (400MHz, CD2Cl2) δ (ppm) 7.95 (d, J = 8.5Hz, 2H), 7.84 (t, J = 8.7Hz, 3H), 7.81-7.76 (m, 3H), 7.68 (d, J = 2.0Hz, 1H) ,7.58-7.49(m,3H),7.43(dd,J=15.3,7.9Hz,8H),7.36(dd,J=14.4,7.3Hz,3H),7.28(t,J=7.4Hz,3H),7.19(q,J=8.1 Hz,3H),7.09(d,J=8.8Hz,1H),7.01(dd,J=8.6,1.9Hz,1H),6.93(d,J=8.8Hz,1H),6.60(dd,J=17.6,10.9Hz,1H),6.2 7(d,J=8.6Hz,1H),6.21(d,J=8.5Hz,1H),5.54(dd,J=17.6,0.7Hz,1H),5.05-5.00(m,1H),1.69(s,3H),1.63(s,3H). 13CNMR (101MHz, CDCl3) δ (ppm) 195.91, 151.57, 151.46, 147.06, 146.93, 145.01, 140.05, 139.48, 137.77, 137.34, 137.27, 136.53, 134. 57,134.42,132.82,132.74,132.12,131.63,131.58,131.15,130.71,130.38,130.35,130.14,130.02,129.91,128.51,128.40,128.3 6,128.28,128.16,127.32,126.91,126.84,126.48,126.45,125.84,125.47,125.28,125.21,125.17,124.35,123.86,121.40,114.42 ,113.89,111.17,36.28,34.72,34.59,31.83,31.66,31.55,29.12,26.97,25.34,22.87,22.73,20.77,14.21,11.52.TOF-MS(ESI)m / z calcd for C 62 H 43 NO3:849.32;[M+H]+found:850.52.
[0060] Synthesis of polymer (R)-E-0.02 / (S)-E-0.02
[0061] Binaphthyl was introduced into the TADF unit, and the chiral TADF unit was suspended on the side chain of the polystyrene skeleton at a feed ratio of 2%. A series of chiral green light TADF polymers were synthesized by free radical polymerization strategy. The specific experimental method is as follows: Compound 7 (17.0 mg, 0.02 mmol), styrene (102.1 mg, 0.98 mmol), azobisisobutyronitrile (0.6 mg, 0.004 mmol), and 0.6 mL of anhydrous tetrahydrofuran were added in sequence to a 25 mL Schlenk bottle. The mixture was first frozen at low temperature (77 K) to remove oxygen, and then N2 was introduced. The operation was repeated three times, and finally heated to 55 ° C under N2 protection for 48 hours. Cooled to room temperature, the mixture was first precipitated with acetone to wash away the monomer and initiator, filtered, and the collected residue was completely dissolved in tetrahydrofuran, and then methanol was added dropwise to precipitate, and a yellow solid was obtained by suction filtration. (R)-E-0.02 was 59.6 mg, (S)-E-0.02 was 65.8 mg, and the yields were 5% and 5%, respectively. 1From the H NMR spectrum, the chemical shift of the hydrogen atom peak in the TADF unit is 7.8-8.0ppm, and the chemical shift of the hydrogen atom peak in the benzene ring region and the hydrogen atom peak of styrene in the TADF unit is 5.8-8.0ppm. The actual content of the TADF unit in the polymer can be determined based on the integral ratio of these two regions. The molar contents of TADF units corresponding to (R)-E-0.02 / (S)-E-0.02 are 2.3% and 2.3%, respectively, which are very close to their feed ratios.
[0062] Synthesis of polymer (R)-E-0.05 / (S)-E-0.05
[0063] Binaphthyl was introduced into the TADF unit, and the chiral TADF unit was suspended on the side chain of the polystyrene skeleton at a feed ratio of 5%, and a series of chiral green light TADF polymers were synthesized by free radical polymerization strategy. The specific experimental method is as follows: Compound 7 (42.5 mg, 0.05 mmol), styrene (98.9 mg, 0.95 mmol), azobisisobutyronitrile (0.6 mg, 0.004 mmol), and 0.7 mL of anhydrous tetrahydrofuran were added in sequence to a 25 mL Schlenk bottle. The mixture was first frozen at low temperature (77 K) to remove oxygen, and then N2 was introduced. The operation was repeated three times, and finally heated to 55 ° C under N2 protection for 48 hours. Cooled to room temperature, the mixture was first precipitated with acetone to wash away the monomer and initiator, filtered, and the collected residue was completely dissolved in tetrahydrofuran, and then methanol was added dropwise to precipitate, and a yellow solid was obtained by suction filtration. The polymer (R)-E-0.05 is 119.6 mg, and (S)-E-0.05 is 109.7 mg, with yields of 5% and 8%, respectively. Similarly, the actual content of TADF units in the polymer can also be determined based on the integral ratio of the two regions. The molar contents of TADF units corresponding to (R)-E-0.05 / (S)-E-0.05 are 5.0% and 5.1%, respectively, which are also very close to their feed ratios.
[0064] Synthesis of polymer (R)-E-0.1 / (S)-E-0.1
[0065] Binaphthyl was introduced into the TADF unit, and the chiral TADF unit was suspended on the side chain of the polystyrene skeleton at a feed ratio of 10%. A series of chiral green light TADF polymers were synthesized by free radical polymerization strategy. The specific experimental method is as follows: Compound 7 (85.0 mg, 0.10 mmol), styrene (93.7 mg, 0.90 mmol), azobisisobutyronitrile (0.6 mg, 0.004 mmol), and 0.9 mL of anhydrous tetrahydrofuran were added in sequence to a 25 mL Schlenk bottle. The mixture was first frozen at low temperature (77 K) to remove oxygen, and then N2 was introduced. The operation was repeated three times, and finally heated to 55 ° C under N2 protection for 48 hours. Cooled to room temperature, the mixture was first precipitated with acetone to wash away the monomer and initiator, filtered, and the collected residue was completely dissolved in tetrahydrofuran, and then methanol was added dropwise to precipitate, and a yellow solid was obtained by suction filtration. The polymer (R)-E-0.1 is 106.5 mg, and (S)-E-0.1 is 95.7 mg, with yields of 11% and 8%, respectively. Similarly, the actual content of TADF units in the polymer can also be determined based on the integral ratio of the two regions. The molar contents of TADF units corresponding to (R)-E-0.1 / (S)-E-0.1 are 10.2% and 10.2%, respectively, which are also very close to their feed ratios.
[0066] Example 2
[0067] The polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 were subjected to gel permeation chromatography using THF as the eluent to determine their molecular weight and PDI. Figure 1 It can be seen that the weight average molecular weight of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 ranges from 11700 to 62600 Da / mol, and the PDI ranges from 1.20 to 1.96.
[0068] Example 3
[0069] The polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 were heated at a rate of 20°C per minute in the range of 30 to 600°C under N2, and the thermogravimetric curves were measured. Figure 2 It can be seen that the temperatures at which polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 decompose by 5% are 381 / 389°C, 380 / 384°C and 395 / 389°C, respectively.
[0070] Example 4
[0071] The polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 were dissolved in acetonitrile solution (10 -5 mol / L) to study its redox characteristics. Figure 3 It can be seen that the irreversible oxidation potential of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 is observed in the range of 0.99eV to 1.10eV, while the reduction potential is not detected in the range of 0 to 2.0V. According to the formula, the HOMO energy level of (R / S)-E-0.02 is -5.35 / -5.32eV, (R / S)-E-0.05 is -5.34 / -5.31eV, (R / S)-E-0.1 is -5.25 / -5.24eV, and the LUMO energy levels are -2.61 / -2.58eV, -2.60 / -2.57eV and -2.51 / -2.50eV, respectively. Obviously, with the increase of the proportion of chiral TADF units, the HOMO and LUMO energy levels gradually increase.
[0072] Example 5
[0073] The polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 were dissolved in toluene to prepare 10 -5 M solution, and test its UV-visible absorption and photoluminescence spectrum. Figure 4 (a) It can be seen that the UV-visible absorption spectra of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in solution have roughly two absorption peaks: the absorption peak at short wavelength (310-350nm) is mainly attributed to the π-π* transition absorption of the material; the absorption peak at long wavelength (400-450nm) is attributed to the charge transfer (ICT) transition absorption peak from the donor unit to the acceptor unit in the polymer. Figure 4 As shown in (a), the maximum emission peaks of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 are about 510 nm, which is in the green light region. Figure 4 (b) is the photoluminescence spectra of all polymers in pure films. The maximum emission peaks of the polymers are in the range of 512-521 nm, which is in the green light region.
[0074] Example 6
[0075] The polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 were prepared to the same concentration (10-5 M) in different proportions of tetrahydrofuran and water mixed solvents, and tested its emission spectrum to study its aggregation-induced emission enhancement characteristics. Figure 5 It can be seen that with the increase of water content, the emission intensity of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 first decreases and then gradually increases. From the dot-line graph of the relationship between emission intensity and water content, it can be clearly seen that as the proportion of water content increases, the polymers aggregate, proving the AIEE properties of this series of polymers.
[0076] Example 7
[0077] The pure films of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 were placed in a low-temperature test kettle, evacuated for 15 minutes, and then slowly added with liquid nitrogen until the temperature dropped to 77K. The fluorescence and phosphorescence spectra were tested using a flash xenon lamp as the excitation light source with an excitation wavelength of 350nm. Figure 6 It can be seen that the ΔE of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 is calculated according to the formula ST The range is 0.16eV-0.19eV, all less than 0.30eV, indicating that it should have TADF properties.
[0078] Example 8
[0079] The fluorescence lifetimes of the polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 in pure films were tested under a nitrogen atmosphere. Figure 7 As shown, after fitting, it is concluded that the instantaneous lifetimes of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 are in the nanosecond level, which are 16.0 / 16.5ns, 17.9 / 16.5ns and 28.0 / 24.6ns, respectively.
[0080] Example 9
[0081] The transient fluorescence spectra of the polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 in pure films were tested under nitrogen atmosphere. Figure 8As shown, the polymers have obvious instantaneous lifetime and delayed lifetime at room temperature. The delayed lifetimes of all polymers show double exponential decay, which is in the microsecond level, namely 14.3μs / 13.1μs, 8.8μs / 11.1μs and 3.0μs / 4.0μs, which indicates that all polymers should have TADF properties.
[0082] Example 10
[0083] The transient fluorescence spectra of the pure films of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 were tested at 100, 200 and 300 K in a nitrogen atmosphere. Fig. 9 As shown, it can be seen that as the temperature increases, the delayed component increases successively, which fully confirms the TADF characteristics of the polymer.
[0084] Embodiment 11
[0085] The polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 were dissolved in toluene to prepare 10 -5 M solution, and tested its circular dichroism absorption (CD) of the solution, and CPL spectrum in pure film state to study its circularly polarized luminescence properties. Fig.10 It can be seen that the CD absorption spectra of all polymers show perfect mirror symmetry, indicating that they are chiral in the ground state; however, no obvious chiral signals were detected in the CPL spectra of pure films of polymers (R) / (S)-E-0.02 and (R) / (S)-E-0.05.
[0086] Example 12
[0087] The polymer (R) / (S)-E-0.1 prepared in Example 1 was dissolved in dichloromethane to prepare 10 -5 M solution, and tested its circular dichroism (CD) absorption and CPL spectrum in pure film state to study its circularly polarized luminescence properties. Fig.11 It can be seen that the CD absorption spectrum of polymer (R) / (S)-E-0.1 shows perfect mirror symmetry, indicating that it has chirality in the ground state; with the increase of the proportion of chiral TADF units, the CPL spectrum of polymer (R) / (S)-E-0.1, which is close to mirror symmetry, reflects the chiral luminescence characteristics of the excited state, and the chiral signal is significantly enhanced. lum | respectively -2.8×10 -3 and +2.6×10 -3 .
[0088] Example 13
[0089] The polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 are used in organic electroluminescent devices. A non-doped OLED device was prepared by solution processing using the polymer as the device light-emitting layer. The device structure is: ITO / PEDOT:PSS (35nm) /
[0090] (R / S)-E-0.02 / (R / S)-E-0.05 / (R / S)-E-0.1(35nm) / TmPyPB(55nm) / LiF(1nm) / Al(120nm). Fig.12 It can be seen that due to the good energy level matching of the device structure, the device achieves a low turn-on voltage. At the same time, the EQE of the polymer (R / S)-E-0.02 was observed. max EQE of polymer (R / S)-E-0.05 is 7.6 / 7.8%; max 5.9 / 6.6%; EQE of polymer (R / S)-E-0.1 max It is 6.1 / 4.0%.
[0091] Embodiment 14
[0092] Application of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 in organic electroluminescent devices. Based on the polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 as chiral acceptors, commercial TAPC (manufacturer: Luminescence Technology Corp. (Lumtec); purity: Sublimed>99.5%) as achiral donor, a doped device was prepared with a doping ratio of 7:3, and the device structure was: ITO / PEDOT:PSS(35nm) / (R / S)-Ex(x=0.02, 0.05 and 0.1):TAPC(7:3)(35nm) / TmPyPB(55nm) / LiF(1nm) / Al(120nm). Fig.13 It can be seen that in addition to the intrinsic emission peak of (R / S)-E-0.1 at about 520nm, the device also forms a new orange-red emission peak at about 580nm. The combined effect of the two can achieve white light emission. As the voltage increases to about 5.6V, the electroluminescence spectrum of the doped device shows an orange-red emission peak at about 580nm, and as the voltage increases, the emission intensity of the orange-red emission peak gradually increases.
[0093] Embodiment 15
[0094] The photoluminescence spectra of the polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 in pure film and 70wt% doped in TAPC film were tested to further prove the origin of the orange-red emission peak. Fig.14 It can be seen that the PL spectra of the polymer film before and after doping with TAPC are basically similar, and the PL spectrum after doping only shows a slight blue shift, which may be caused by the weakening of the intermolecular force of the polymer (R / S)-E-0.1 after doping with TAPC. The newly formed peak in the EL spectrum is not observed in the PL spectrum of the blend film of the donor and acceptor molecules, which is consistent with the definition of the electroexciton complex and proves the source of white light emission.
[0095] Example 16
[0096] Application of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 in organic electroluminescent devices. Based on the polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 prepared in Example 1 as chiral acceptors and commercial TAPC as achiral donor, doped devices were prepared with doping ratios of 5:5, 7:3 and 9:1. The device structure was: ITO / PEDOT:PSS(35nm) / (R / S)-Ex(x=0.02, 0.05 and 0.1):TAPC(5:5, 7:3 and 9:1)(35nm) / TmPyPB(55nm) / LiF(1nm) / Al(120nm). Fig.15 It can be seen that white light emission is achieved due to the formation of orange-red electroexciton complexes between the polymer and TAPC in the light-emitting layer. When the doping ratio of polymer (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 to TAPC is 5:5, the EQE of the device prepared based on (R / S)-E-0.02:TAPC as the light-emitting layer is max 11.0 / 10.6%; (R / S)-E-0.05: EQE of TAPC max 6.7 / 6.8%; (R / S)-E-0.1: EQE of TAPC max When the doping ratio of polymer (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 to TAPC is 7:3, the EQE of the device prepared based on (R / S)-E-0.02:TAPC as the light-emitting layer is max 13.6 / 16.2%; (R / S)-E-0.05: EQE of TAPCmax 8.0 / 8.2%; (R / S)-E-0.1: EQE of TAPC max When the doping ratio of polymer (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 to TAPC is 9:1, the EQE of the device prepared based on (R / S)-E-0.02:TAPC as the light-emitting layer is max 9.2 / 14.4%; (R / S)-E-0.05: EQE of TAPC max 6.4 / 7.0%; (R / S)-E-0.1: EQE of TAPC max The device achieved the maximum external quantum efficiency when the doping ratio of polymer (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 and TAPC was 7:3.
[0097] Embodiment 17
[0098] Based on the polymer (R) / (S)-E-0.1 prepared in Example 1 as a chiral acceptor and commercial TAPC as an achiral donor, a white electroexcimer type device was prepared with an acceptor and donor optimal device efficiency doping ratio of 7:3 to study its circularly polarized electroluminescent performance. Fig.16 It can be seen that the broad and mirror-symmetric electro-induced circularly polarized luminescence spectrum exhibited by the device reflects its circularly polarized electroluminescence characteristics. (R) / (S)-E-0.1:|g of TAPC EL | respectively -1.0×10 -3 and +1.0×10 -3 .
[0099] Embodiment 18
[0100] The polymer (R) / (S)-E-0.170wt% prepared in Example 1 was doped into TAPC to prepare a doped film and its CPL spectrum was tested to study its circularly polarized luminescence properties. Fig.17 It can be seen that the CPL spectrum of (R) / (S)-E-0.1:TAPC, which is close to mirror symmetry, reflects the circularly polarized luminescence characteristics. lum | respectively -2.4×10 -3 and +2.0×10 -3 .
[0101] Embodiment 19
[0102] Application of polymers (R) / (S)-E-0.02, (R) / (S)-E-0.05 and (R) / (S)-E-0.1 in Example 1 in organic electroluminescent devices. Based on the electroluminescent complex formed by the polymer (R) / (S)-E-0.1 and TAPC prepared in Example 1 as the guest, CBP as the host of the white light electroluminescent complex, and doping devices with doping ratios of host and guest of 5:5, 3:7 and 1:9 respectively. The device structure is: ITO / PEDOT:PSS(35nm) / CBP:((R / S)-E-0.1:TAPC(7:3))(5:5, 3:7 and 1:9)(35nm) / TmPyPB(55nm) / LiF(1nm) / Al(120nm). Fig.18 It can be seen that the device performance is further improved through the effective FRET energy transfer between the host and the guest. When the CBP:((R / S)-E-0.1:TAPC) doping ratio is 5:5, the EQE of the device prepared based on CBP:((R / S)-E-0.1:TAPC) as the light-emitting layer is max When the CBP:((R / S)-E-0.1:TAPC) doping ratio is 3:7, the EQE of the device prepared based on CBP:((R / S)-E-0.1:TAPC) as the light-emitting layer is 13.8 / 14.0%. max When the CBP:((R / S)-E-0.1:TAPC) doping ratio is 1:9, the EQE of the device prepared based on CBP:((R / S)-E-0.1:TAPC) as the light-emitting layer is max The device achieved the maximum external quantum efficiency when the CBP:((R / S)-E-0.1:TAPC) doping ratio was 3:7.
[0103] Embodiment 20
[0104] Based on the electroexcimer complex formed by the polymer (R) / (S)-E-0.1 and TAPC prepared in Example 1 as the guest, CBP as the host of the white light electroexcimer complex, a white electroexcimer complex type device was prepared with the best device efficiency doping ratio of host and guest of 3:7 to study its circularly polarized electroluminescent performance. Fig.19 It can be seen that the broad and mirror-symmetric electro-induced circularly polarized luminescence spectrum of the device reflects its circularly polarized electroluminescence characteristics. CBP: ((R / S)-E-0.1:TAPC) |g EL | respectively -1.8×10 -3 and +2.4×10 -3 .
[0105] Embodiment 21
[0106] 70 wt% of the electroexciton complex formed by the polymer (R) / (S)-E-0.1 and TAPC prepared in Example 1 was doped into CBP to prepare a doped film and its CPL spectrum was tested to study its circularly polarized luminescence properties. Fig. 20 It can be seen that the CPL spectrum of CBP: ((R / S)-E-0.1: TAPC) is nearly mirror-symmetrical, reflecting the circularly polarized luminescence characteristics. lum | respectively -3.0×10 -3 and +2.4×10 -3 .
[0107] Although the present invention has been described in conjunction with the preferred embodiments, the present invention is not limited to the above embodiments, and it should be understood that the appended claims summarize the scope of the present invention. Under the guidance of the inventive concept, those skilled in the art should be aware that certain changes made to the various embodiments of the present invention will be covered by the spirit and scope of the claims of the present invention.
Claims
1. A chiral thermally activated delayed fluorescent polymer, characterized in that: The molecular structure of the chiral thermally activated delayed fluorescent polymer is as follows:
2. A method for preparing a chiral thermally activated delayed fluorescent polymer according to claim 1, characterized in that: The preparation method comprises the following steps: using a binaphthyl derivative as a chiral source, benzophenone as an electron acceptor, and acridine as an electron donor, directly introducing the binaphthyl chiral source into a TADF unit, suspending it on a polystyrene skeleton side chain, and synthesizing a series of chiral green photothermally activated delayed fluorescent polymers by adjusting the ratio of the TADF unit during polymerization and adopting a non-conjugated polymerization strategy.
3. The chiral thermally activated delayed fluorescent polymer according to claim 1, characterized in that: The binaphthyl derivative is (R / S)-binaphthol.
4. The chiral thermally activated delayed fluorescent polymer according to claim 1, characterized in that: The proportion of the chiral TADF unit is 2%-10%.
5. A use of the chiral thermally activated delayed fluorescent polymer according to claim 1, characterized in that: The chiral thermally activated delayed fluorescence polymer is used for preparing a white circularly polarized organic light emitting diode.
6. The use of the chiral thermally activated delayed fluorescent polymer according to claim 5, characterized in that: The light-emitting layer of a white circularly polarized organic light-emitting diode is prepared by a solution processing method using a chiral thermally activated delayed fluorescent polymer as a light-emitting layer or a light-emitting layer dopant.
7. The use of the chiral thermally activated delayed fluorescent polymer according to claim 6, characterized in that: The external quantum efficiency of a white circularly polarized organic light-emitting diode prepared by using a chiral thermally activated delayed fluorescent polymer as a light-emitting layer or a light-emitting layer dopant is 10.8-15.1%.
8. The use of the chiral thermally activated delayed fluorescent polymer according to claim 6, characterized in that: The chiral thermally activated delayed fluorescent polymer is used as a dopant in the light-emitting layer to prepare a white circularly polarized organic light-emitting diode, and the doping mass percentage is 50-90wt%.
Citation Information
Patent Citations
Near-infrared thermal activation delayed fluorescence luminescent material based on dicyanophenene and application of near-infrared thermal activation delayed fluorescence luminescent material
CN115490631A
High-efficiency chiral liquid crystal fluorescent material and application thereof
CN115745885A
Chiral luminescent material with space charge transfer effect and application thereof
CN117143320A
Method of making fluorescent compound bonded-polymers and polymers made thereby
US3462388A
Chiral thermally activated delayed fluorescence material and preparation method therefor
WO2022052135A1