Graphene high-absorptivity resin and preparation method thereof

By using potassium persulfate and acrylamide monomers in the preparation of graphene hyperabsorbent resin, the preparation steps of graphene hyperabsorbent resin are optimized, the problem of insufficient salt resistance is solved, and the absorption of resin is improved. Recycling life.

CN118909210APending Publication Date: 2024-11-08SATELLITE SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410929143.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Graphene high-absorbent resin has poor salt resistance when contacting salt liquid, which affects its water absorption and service life and reduces its reusable performance.

Method used

Potassium persulfate is used as the initiator during the preparation of graphene hyperabsorbent resin, and acrylamide monomer and cyclohexane are added to optimize the preparation steps to improve the absorption and salt resistance of the resin.

Benefits of technology

The recycling life of graphene high-absorbent resin is improved, and the raw material mixing and drying during the preparation process is optimized, ensuring the quality and salt resistance of the resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909210A_ABST
    Figure CN118909210A_ABST
Patent Text Reader

Abstract

The invention discloses graphene high-absorptivity resin and a preparation method thereof. The graphene high-absorptivity resin is prepared from the following raw materials in parts by weight: a high-absorptivity resin material, graphene oxide powder, a potassium sulfate initiator, a cross-linking agent, a filling agent, a water-resistant agent, a tackifier, acrylic acid, an acrylamide monomer, cyclohexane, a sodium hydroxide solution, a dispersing agent, an anti-aging agent and a curing agent. Preparation steps of the graphene high-absorptivity resin are optimized and improved, potassium persulfate is used as an initiator in a material prepared from the graphene high-absorptivity resin, and an acrylamide monomer and cyclohexane are added for blending, so that the graphene high-absorptivity resin keeps relatively good absorptivity and salt tolerance; the cyclic utilization life of the graphene high-absorptivity resin is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resin preparation, and in particular to a graphene high-absorbency resin and a preparation method thereof. Background Art

[0002] Super absorbent resin is a new type of functional polymer material with a three-dimensional network structure that is moderately cross-linked by a cross-linking agent. It is usually called "water retaining agent", "super absorbent polymer", "super absorbent", etc. Since super absorbent resin contains strong hydrophilic groups, such as carboxyl, amide, ester, etc., it can quickly absorb dozens or even thousands of times its own weight of water or dozens of times of salt solution through hydration to form a gel, and has good water retention performance. Therefore, it is widely used in agriculture, forestry, horticulture, desert control, medical care, civil engineering, food processing, petrochemical and other fields; and graphene super absorbent resin is a new type of synthetic resin that adds graphene to the synthetic resin to improve the properties of the resin.

[0003] At present, in the actual use process of graphene high absorbent resin, graphene high absorbent resin will easily come into contact with some saline liquids, and the existing graphene high absorbent resin has poor salt resistance, which affects the water absorption performance of the graphene high absorbent resin in subsequent use, and the service life of the graphene high absorbent resin will also be affected, thereby reducing the reusability of the graphene high absorbent resin. For this reason, we propose a graphene high absorbent resin and a preparation method thereof. Summary of the invention

[0004] The main purpose of the present invention is to provide a graphene high-absorbency resin and a preparation method thereof. The present invention optimizes and improves the preparation steps of the graphene high-absorbency resin, uses potassium persulfate as an initiator in the material prepared from the graphene high-absorbency resin, and adds acrylamide monomer and cyclohexane for blending, so that the graphene high-absorbency resin maintains good absorbency and salt resistance, improves the recycling life of the graphene high-absorbency resin, and can effectively solve the problems in the background technology.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A graphene high-absorbency resin and a preparation method thereof, comprising the graphene high-absorbency resin being composed of the following raw materials in parts by weight:

[0007] 60-120 parts of high-absorbent resin material, 5-15 parts of graphene oxide powder, 4-12 parts of potassium sulfate initiator, 4-15 parts of cross-linking agent, 4-15 parts of filler, 4-15 parts of water-resistant agent, 4-15 parts of tackifier, 4-20 parts of acrylic acid, 4-20 parts of acrylamide monomer, 4-15 parts of cyclohexane, 3-18 parts of sodium hydroxide solution, 3-10 parts of dispersant, 3-15 parts of antioxidant and 6-12 parts of curing agent;

[0008] The preparation method of the above-mentioned graphene high absorbent resin comprises the following steps:

[0009] S1, taking 6 parts of cyclohexane and 8 parts of dispersant, putting them into an external stirring container and mixing at room temperature to prepare an oil phase;

[0010] S2, in a water bath container under normal temperature conditions, 5 parts of sodium hydroxide solution of a certain concentration are mixed with 10 parts of acrylic acid for neutralization, and after the 10 parts of acrylic acid reach the required neutralization degree, 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added in sequence and stirred evenly to obtain an aqueous phase;

[0011] S3, adding 75 parts of high-absorbent resin material, 15 parts of graphene oxide powder, 6 parts of filler, 12 parts of water-resistant agent and 11 parts of antioxidant into a reactor, heating the materials in the reactor to 70° C. and stirring, and subsequently adding 10 parts of tackifier and stirring to obtain a resin mixture;

[0012] The oil phase in S4 and S1, the water phase in S2 and 10 parts of curing agent are added into the reactor and mixed with the resin mixture. At this time, the reactor is heated to 70° C. again to stir and mix the materials. 4 parts of potassium sulfate initiator and 8 parts of cross-linking agent undergo polymerization reaction between the graphene oxide powder layers in the resin mixture to form a cross-linking structure in situ. Then, a certain stirring treatment is performed to form a graphene high-absorption resin base material.

[0013] S5, the graphene high-absorbent resin base material is taken out from the reactor and cleaned with a cleaning agent, and then the graphene high-absorbent resin base material is sent to a drying oven for drying after cleaning, and the dried graphene high-absorbent resin base material is crushed by a crusher to obtain a graphene high-absorbent resin;

[0014] The water bath container described in S2 includes a base, a main box, an auxiliary box, a water pump, a box connecting pipe, a bucket box and a frame seat. The main box and the auxiliary box are symmetrically welded on the surface of the base, and a connecting plate for supporting the water pump is welded between the box walls on one side of the main box and the auxiliary box. The water inlet flange of the water pump is connected with a water pipe extending into the main box to pump water, and the water outlet flange of the water pump is connected with a drainage pipe extending into the auxiliary box for drainage. The box walls on the other side of the main box and the auxiliary box away from the connecting plate are interconnected by a box connecting pipe, and a bucket box with a bottom welded frame seat is placed in the main box and the auxiliary box.

[0015] Among them, 5 parts of sodium hydroxide solution and 10 parts of acrylic acid in S2 are mixed and neutralized in a bucket box, and then 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added to the bucket box in sequence and stirred evenly to obtain an aqueous phase;

[0016] By adopting the above technical scheme, 5 parts of sodium hydroxide solution and 10 parts of acrylic acid in S2 can be neutralized in a bucket box under a normal temperature water bath state, and the subsequent addition of 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent can also be maintained under a normal temperature water bath environment to produce a high-quality aqueous phase.

[0017] The box body of the bucket box is a metal box body with good thermal conductivity, and four sets of seat rods of the frame seat are welded outside the lower box body of the bucket box;

[0018] By adopting the above technical solution, the bucket box can conduct heat well after being placed in the water-filled main box 2 and auxiliary box 3 with a frame seat, so that the bucket box can maintain a normal temperature at the water temperature during the water bath.

[0019] Wherein, the box connecting pipes are welded in two groups between the main box and the auxiliary box;

[0020] By adopting the above technical solution, the main box and the auxiliary box are interconnected by a double set of box connecting pipes.

[0021] The graphene high-absorption resin base material in S5 is dried at a temperature of 80°C in the drying oven, and is naturally cooled to room temperature after being dried in the drying oven at 80°C;

[0022] By adopting the above technical solution, the block drying process of the graphene high-absorbency resin base material in S5 is relatively stable.

[0023] Wherein, the graphene high-absorption resin base material in S5 can be cut into small pieces for drying when drying in a drying oven;

[0024] By adopting the above technical solution, the graphene high-absorbency resin base material in S5 can be dried efficiently in small pieces.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The present invention optimizes and improves the preparation steps of the graphene super absorbent resin, uses potassium persulfate as an initiator in the material prepared from the graphene super absorbent resin, and adds acrylamide monomer and cyclohexane for blending, so that the graphene super absorbent resin maintains good absorbency and salt resistance, thereby improving the recycling life of the graphene super absorbent resin.

[0027] 2. The present invention provides a water bath container for a normal temperature water bath in the preparation step of the graphene super absorbent resin to meet the neutralization and mixing requirements of the sodium hydroxide solution, acrylic acid, acrylamide monomer, potassium sulfate initiator and cross-linking agent, thereby ensuring the quality of the aqueous phase raw material for preparing the graphene super absorbent resin, and further optimizing the quality of the graphene super absorbent resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a schematic diagram of a water bath container structure of a graphene high absorbent resin and a preparation method thereof.

[0029] Figure 2 This is an exploded view of a water bath container of a graphene high absorbent resin and a preparation method thereof according to the present invention.

[0030] In the figure: 1. base; 2. main box; 3. auxiliary box; 4. connecting plate; 5. water pump; 6. water inlet pipe; 7. drainage pipe; 8. box connecting pipe; 9. bucket box; 10. frame base. DETAILED DESCRIPTION

[0031] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0032] Embodiment 1

[0033] like Figure 1-2 As shown, a graphene high absorbent resin and a preparation method thereof, comprising the graphene high absorbent resin consisting of the following raw materials in parts by weight:

[0034] 60-120 parts of high-absorbent resin material, 5-15 parts of graphene oxide powder, 4-12 parts of potassium sulfate initiator, 4-15 parts of cross-linking agent, 4-15 parts of filler, 4-15 parts of water-resistant agent, 4-15 parts of tackifier, 4-20 parts of acrylic acid, 4-20 parts of acrylamide monomer, 4-15 parts of cyclohexane, 3-18 parts of sodium hydroxide solution, 3-10 parts of dispersant, 3-15 parts of antioxidant and 6-12 parts of curing agent;

[0035] The preparation method of the above-mentioned graphene high absorbent resin comprises the following steps:

[0036] S1, taking 6 parts of cyclohexane and 8 parts of dispersant, putting them into an external stirring container and mixing at room temperature to prepare an oil phase;

[0037] S2, in a water bath container under normal temperature conditions, 5 parts of sodium hydroxide solution of a certain concentration are mixed with 10 parts of acrylic acid for neutralization, and after the 10 parts of acrylic acid reach the required neutralization degree, 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added in sequence and stirred evenly to obtain an aqueous phase;

[0038] S3, adding 75 parts of high-absorbent resin material, 15 parts of graphene oxide powder, 6 parts of filler, 12 parts of water-resistant agent and 11 parts of antioxidant into a reactor, heating the materials in the reactor to 70° C. and stirring, and subsequently adding 10 parts of tackifier and stirring to obtain a resin mixture;

[0039] The oil phase in S4 and S1, the water phase in S2 and 10 parts of curing agent are added into the reactor and mixed with the resin mixture. At this time, the reactor is heated to 70° C. again to stir and mix the materials. 4 parts of potassium sulfate initiator and 8 parts of cross-linking agent undergo polymerization reaction between the graphene oxide powder layers in the resin mixture to form a cross-linking structure in situ. Then, a certain stirring treatment is performed to form a graphene high-absorption resin base material.

[0040] S5, the graphene high-absorbent resin base material is taken out from the reactor and cleaned with a cleaning agent, and then the graphene high-absorbent resin base material is sent to a drying oven for drying after cleaning, and the dried graphene high-absorbent resin base material is crushed by a crusher to obtain a graphene high-absorbent resin;

[0041] The water bath container described in S2 includes a base 1, a main box 2, an auxiliary box 3, a water pump 5, a box connecting pipe 8, a bucket box 9 and a frame seat 10. The main box 2 and the auxiliary box 3 are symmetrically welded on the surface of the base 1, and a connecting plate 4 for supporting the water pump 5 is welded between the box walls on one side of the main box 2 and the auxiliary box 3. The water inlet flange of the water pump 5 is connected with a water diversion pipe 6 extending into the main box 2 to pump water, and the water outlet flange of the water pump 5 is connected with a drainage pipe 7 extending into the auxiliary box 3 to drain water. The box connecting pipe 8 is welded to each other between the box walls on the other side of the main box 2 and the auxiliary box 3 away from the connecting plate 4, and a bucket box 9 with a bottom welded frame seat 10 is placed in the main box 2 and the auxiliary box 3.

[0042] Among them, 5 parts of sodium hydroxide solution and 10 parts of acrylic acid in S2 are mixed and neutralized in the bucket box 9, and then 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added to the bucket box 9 in sequence and stirred evenly to obtain an aqueous phase;

[0043] By adopting the above technical scheme, 5 parts of sodium hydroxide solution and 10 parts of acrylic acid in S2 can be neutralized in the bucket box 9 under the normal temperature water bath state, and the subsequent addition of 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent can also be maintained under the normal temperature water bath environment to produce a high-quality aqueous phase.

[0044] The box body of the bucket box 9 is a metal box body with good thermal conductivity, and four sets of seat rods of the frame seat 10 are welded outside the lower box body of the bucket box 9;

[0045] By adopting the above technical solution, the bucket box 9 can conduct heat well after being placed in the water-filled main box 2 and auxiliary box 3 with the frame seat 10, so that the bucket box 9 can maintain a normal temperature with the water temperature during the water bath.

[0046] Among them, the box connecting pipes 8 are welded in two groups between the main box 2 and the auxiliary box 3;

[0047] By adopting the above technical solution, the main tank 2 and the auxiliary tank 3 are interconnected by a double set of tank connecting pipes 8 .

[0048] The graphene high-absorption resin base material in S5 is dried at a temperature of 80°C in the drying oven, and is naturally cooled to room temperature after being dried in the drying oven at 80°C;

[0049] By adopting the above technical solution, the block drying process of the graphene high-absorbency resin base material in S5 is relatively stable.

[0050] Wherein, the graphene high-absorption resin base material in S5 can be cut into small pieces for drying when drying in a drying oven;

[0051] By adopting the above technical solution, the graphene high-absorbency resin base material in S5 can be dried efficiently in small pieces.

[0052] Embodiment 2

[0053] like Figure 1-2 As shown, a graphene high absorbent resin and a preparation method thereof, comprising the graphene high absorbent resin consisting of the following raw materials in parts by weight:

[0054] 60-120 parts of high-absorbent resin material, 5-15 parts of graphene oxide powder, 4-12 parts of potassium sulfate initiator, 4-15 parts of cross-linking agent, 4-15 parts of filler, 4-15 parts of water-resistant agent, 4-15 parts of tackifier, 4-20 parts of acrylic acid, 4-20 parts of acrylamide monomer, 4-15 parts of cyclohexane, 3-18 parts of sodium hydroxide solution, 3-10 parts of dispersant, 3-15 parts of antioxidant and 6-12 parts of curing agent;

[0055] The preparation method of the above-mentioned graphene high absorbent resin comprises the following steps:

[0056] S1, taking 7 parts of cyclohexane and 9 parts of dispersant, putting them into an external stirring container and mixing at room temperature to prepare an oil phase;

[0057] S2, in a water bath container under normal temperature conditions, 5 parts of sodium hydroxide solution of a certain concentration are mixed with 10 parts of acrylic acid for neutralization, and after the 10 parts of acrylic acid reach the required neutralization degree, 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added in sequence and stirred evenly to obtain an aqueous phase;

[0058] S3, adding 80 parts of high-absorbent resin material, 15 parts of graphene oxide powder, 6 parts of filler, 12 parts of water-resistant agent and 11 parts of antioxidant into a reactor, heating the materials in the reactor to 60° C. and stirring, and subsequently adding 11 parts of tackifier and stirring to obtain a resin mixture;

[0059] The oil phase in S4 and S1, the water phase in S2 and 12 parts of curing agent are added into the reactor and mixed with the resin mixture. At this time, the reactor is heated to 70° C. again to stir and mix the materials. 4 parts of potassium sulfate initiator and 8 parts of cross-linking agent undergo polymerization reaction between the graphene oxide powder layers in the resin mixture to form a cross-linking structure in situ. Then, a certain stirring treatment is performed to form a graphene high-absorption resin base material.

[0060] S5, the graphene high-absorbent resin base material is taken out from the reactor and cleaned with a cleaning agent, and then the graphene high-absorbent resin base material is sent to a drying oven for drying after cleaning, and the dried graphene high-absorbent resin base material is crushed by a crusher to obtain a graphene high-absorbent resin;

[0061] The water bath container described in S2 includes a base 1, a main box 2, an auxiliary box 3, a water pump 5, a box connecting pipe 8, a bucket box 9 and a frame seat 10. The main box 2 and the auxiliary box 3 are symmetrically welded on the surface of the base 1, and a connecting plate 4 for supporting the water pump 5 is welded between the box walls on one side of the main box 2 and the auxiliary box 3. The water inlet flange of the water pump 5 is connected with a water diversion pipe 6 extending into the main box 2 to pump water, and the water outlet flange of the water pump 5 is connected with a drainage pipe 7 extending into the auxiliary box 3 to drain water. The box connecting pipe 8 is welded to each other between the box walls on the other side of the main box 2 and the auxiliary box 3 away from the connecting plate 4, and a bucket box 9 with a bottom welded frame seat 10 is placed in the main box 2 and the auxiliary box 3.

[0062] Among them, 5 parts of sodium hydroxide solution and 10 parts of acrylic acid in S2 are mixed and neutralized in the bucket box 9, and then 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added to the bucket box 9 in sequence and stirred evenly to obtain an aqueous phase;

[0063] By adopting the above technical scheme, 5 parts of sodium hydroxide solution and 10 parts of acrylic acid in S2 can be neutralized in the bucket box 9 under the normal temperature water bath state, and the subsequent addition of 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent can also be maintained under the normal temperature water bath environment to produce a high-quality aqueous phase.

[0064] The box body of the bucket box 9 is a metal box body with good thermal conductivity, and four sets of seat rods of the frame seat 10 are welded outside the lower box body of the bucket box 9;

[0065] By adopting the above technical solution, the bucket box 9 can conduct heat well after being placed in the water-filled main box 2 and auxiliary box 3 with the frame seat 10, so that the bucket box 9 can maintain a normal temperature with the water temperature during the water bath.

[0066] Among them, the box connecting pipes 8 are welded in two groups between the main box 2 and the auxiliary box 3;

[0067] By adopting the above technical solution, the main tank 2 and the auxiliary tank 3 are interconnected by a double set of tank connecting pipes 8 .

[0068] The graphene high-absorption resin base material in S5 is dried at a temperature of 80°C in the drying oven, and is naturally cooled to room temperature after being dried in the drying oven at 80°C;

[0069] By adopting the above technical solution, the block drying process of the graphene high-absorbency resin base material in S5 is relatively stable.

[0070] Wherein, the graphene high-absorption resin base material in S5 can be cut into small pieces for drying when drying in a drying oven;

[0071] By adopting the above technical solution, the graphene high-absorbency resin base material in S5 can be dried efficiently in small pieces.

[0072] It should be noted that the present invention is a graphene high absorbency resin and a preparation method thereof. The components in the present invention are all components known to those skilled in the art, and their structures and principles are all known to those skilled in the art through technical manuals or through conventional experimental methods.

[0073] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a graphene high absorbent resin, Features: The graphene high-absorbency resin is composed of the following raw materials in parts by weight: 60-120 parts of high-absorbent resin material, 5-15 parts of graphene oxide powder, 4-12 parts of potassium sulfate initiator, 4-15 parts of cross-linking agent, 4-15 parts of filler, 4-15 parts of water-resistant agent, 4-15 parts of tackifier, 4-20 parts of acrylic acid, 4-20 parts of acrylamide monomer, 4-15 parts of cyclohexane, 3-18 parts of sodium hydroxide solution, 3-10 parts of dispersant, 3-15 parts of antioxidant and 6-12 parts of curing agent; The preparation method of the above-mentioned graphene high absorbent resin comprises the following steps: S1, taking 6 parts of cyclohexane and 8 parts of dispersant, putting them into an external stirring container and mixing at room temperature to prepare an oil phase; S2, in a water bath container under normal temperature conditions, 5 parts of sodium hydroxide solution of a certain concentration are mixed with 10 parts of acrylic acid for neutralization, and after the 10 parts of acrylic acid reach the required neutralization degree, 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added in sequence and stirred evenly to obtain an aqueous phase; S3, adding 75 parts of high-absorbent resin material, 15 parts of graphene oxide powder, 6 parts of filler, 12 parts of water-resistant agent and 11 parts of antioxidant into a reactor, heating the materials in the reactor to 70° C. and stirring, and subsequently adding 10 parts of tackifier and stirring to obtain a resin mixture; The oil phase in S4 and S1, the water phase in S2 and 10 parts of curing agent are added into the reactor and mixed with the resin mixture. At this time, the reactor is heated to 70° C. again to stir and mix the materials. 4 parts of potassium sulfate initiator and 8 parts of cross-linking agent undergo polymerization reaction between the graphene oxide powder layers in the resin mixture to form a cross-linking structure in situ. Then, a certain stirring treatment is performed to form a graphene high-absorption resin base material. S5, the graphene high-absorbent resin base material is taken out from the reactor and cleaned with a cleaning agent, and then the graphene high-absorbent resin base material is sent to a drying oven for drying after cleaning, and the dried graphene high-absorbent resin base material is crushed by a crusher to obtain a graphene high-absorbent resin; The water bath container described in S2 comprises a base (1), a main box (2), an auxiliary box (3), a water pump (5), a box connecting pipe (8), a bucket box (9) and a frame seat (10). The main box (2) and the auxiliary box (3) are symmetrically welded on the surface of the base (1), and a connecting plate (4) for supporting the water pump (5) is welded between the box walls on one side of the main box (2) and the auxiliary box (3). The water inlet flange of the water pump (5) is connected to a water diversion pipe (6) extending into the main box (2) to pump water, and the water outlet flange of the water pump (5) is connected to a drainage pipe (7) extending into the auxiliary box (3) to drain water. The box connecting pipe (8) is welded between the box walls on the other side of the main box (2) and the auxiliary box (3) away from the connecting plate (4), and a bucket box (9) with a bottom welded frame seat (10) is placed in the main box (2) and the auxiliary box (3).

2. A method for preparing a graphene high absorbent resin according to claim 1, Features: 5 parts of the sodium hydroxide solution and 10 parts of acrylic acid in the S2 are mixed and neutralized in a bucket box (9), and then 8 parts of acrylamide monomer, 4 parts of potassium sulfate initiator, and 8 parts of cross-linking agent are added to the bucket box (9) in sequence and stirred evenly to obtain an aqueous phase.

3. A method for preparing a graphene high absorbent resin according to claim 2, Features: The box body of the bucket box (9) is a metal box body with good thermal conductivity, and four groups of seat rods of the frame seat (10) are welded outside the lower box body of the bucket box (9).

4. A method for preparing a graphene high absorbent resin according to claim 1, Features: The tank connecting pipes (8) are welded in two groups between the main tank (2) and the auxiliary tank (3).

5. A method for preparing a graphene high absorbent resin according to claim 1, Features: The drying temperature of the graphene high-absorption resin base material in the drying oven in S5 is 80° C., and after being dried in the drying oven at 80° C., the temperature naturally drops to room temperature.

6. A method for preparing a graphene high absorbent resin according to claim 1, Features: The graphene high-absorption resin base material in S5 can be cut into small pieces for drying when being dried in a drying oven.