Room-temperature self-repairing waterborne polyurethane film as well as preparation method and application thereof
By adding specific compounds and modified two-dimensional MXene materials to the aqueous polyurethane materials, a gradient hydrogen bond network is formed, which solves the problem of balance between self-repair performance and mechanical properties of aqueous polyurethane materials, and achieves rapid self-repair and water resistance at room temperature, which is suitable for Wearable devices.
Patent Information
- Application Number
- CN202411135210.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing water-based polyurethane materials are difficult to balance between achieving good self-repair performance, mechanical properties and water resistance, and the self-repair process is complicated and prone to failure due to water exposure.
By adding diisocyanate compounds, amine compounds and multiple hydrogen bond chain extenders to the mixing of polyether polyols and chain extenders, and mixing them with a modified two-dimensional MXene material, a room temperature self-healing water property with a gradient hydrogen bond network is formed. Polyurethane film, adjusting hydrogen bond ratio for rapid self-healing and good mechanical properties.
It achieves rapid self-healing at room temperature, maintains excellent mechanical properties and water resistance, is suitable for wearable devices, and can maintain good sensing performance after soaking sweat.
Smart Images

Figure CN118909282A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane materials, and in particular to a room temperature self-repairing waterborne polyurethane film and a preparation method and application thereof. Background Art
[0002] Polyurethane is currently widely used in various leathers and coatings due to its excellent mechanical properties and good weather resistance. However, it is difficult to avoid the release of volatile organic gases during the synthesis of polyurethane. In order to solve this problem, water-based polyurethanes that use water as a dispersant and whose synthesis process is more in line with sustainable development have attracted much attention. However, water-based polyurethanes have the defect of being easily damaged during use. At present, there have been studies on the introduction of dynamic chemical bonds to give water-based polyurethanes self-healing ability, but it is difficult to achieve a good balance between self-healing ability and mechanical properties in the existing technology: the introduction of too strong dynamic chemical bonds will greatly hinder the migration of water-based polyurethane segments, thereby greatly reducing the self-healing ability, and the low dynamic bond energy cannot provide sufficient rigidity for water-based polyurethanes. It is necessary to achieve the regulation of dynamic chemical bonds in water-based polyurethanes by simple methods. For self-healing water-based polyurethanes, introducing additional heat to stimulate the self-healing of water-based polyurethanes will greatly increase the complexity of material use, and water-based polyurethane materials are prone to failure when exposed to water. Providing a water-based polyurethane that can achieve rapid self-healing at room temperature and has both excellent mechanical properties and good water resistance is of great significance for simplifying the repair steps and enhancing the durability of materials. Summary of the invention
[0003] The purpose of the present invention is to provide a room temperature self-healing waterborne polyurethane film and a preparation method and application thereof, so as to solve the technical problem that the good self-healing performance, mechanical properties and water resistance of waterborne polyurethane materials in the prior art cannot be balanced.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a method for preparing a room temperature self-repairing waterborne polyurethane film, comprising the following steps:
[0006] 1) mixing a polyether polyol and a chain extender, drying the mixture, and then adding a diisocyanate compound to carry out a polymerization reaction;
[0007] 2) adding a small molecule diol chain extender to the reaction system in step 1) to continue the reaction, and using an organic solvent to adjust the viscosity of the system;
[0008] 3) adding an amine compound to the reaction system of step 2) for neutralization reaction, and then adding a multi-hydrogen bond chain extender for dispersion to obtain a self-healing waterborne polyurethane dispersion;
[0009] 4) The dispersion obtained in step 3) is subjected to rotary evaporation and then mixed with the modified two-dimensional MXene material, and the obtained mixture is placed in a mold and dried to obtain a room temperature self-healing waterborne polyurethane film.
[0010] Furthermore, the mass ratio of the polyether polyol, the chain extender and the diisocyanate compound is 8-12:1:5-7;
[0011] The mass ratio of the chain extender, the small molecule diol chain extender and the amine compound is 1:0.7-1.2:0.6-1;
[0012] The mass ratio of the chain extender, the multiple hydrogen bond chain extender and the modified two-dimensional MXene material is 1:0.4~0.8:0.001~0.03.
[0013] Further, in step 1), the polyether polyol includes polypropylene glycol 2000 and / or polytetrahydrofuran diol;
[0014] The chain extender includes 2,2-dimethylol propionic acid and / or 2,2-dimethylol butyric acid;
[0015] The diisocyanate compound includes isophorone diisocyanate and / or hexamethylene diisocyanate.
[0016] Furthermore, in step 1), the drying temperature is 100 to 130° C., and the drying time is 1.5 to 3 hours;
[0017] The polymerization reaction temperature is 82-100° C., and the polymerization reaction time is 2.5-4 hours;
[0018] The small molecule diol chain extender includes 1,4-butanediol, and the organic solvent includes anhydrous butanone;
[0019] The reaction temperature is 70-80°C and the reaction time is 2-5h;
[0020] The viscosity of the system is in the range of 30 to 60 mPa / s -1 .
[0021] Further, in step 3), the amine compound includes triethylamine;
[0022] The neutralization reaction temperature is 30-40°C, and the neutralization reaction time is 20-40 minutes;
[0023] The multiple hydrogen bond chain extender includes adipic acid dihydrazide and / or N,N-bis(2-hydroxyethyl)oxalamide.
[0024] Furthermore, in step 3), the dispersion speed is 700-1000 rpm, and the dispersion time is 0.5-2 h.
[0025] Furthermore, in step 3), the mixing temperature is 20-40° C., and the mixing time is 0.5-2 h; the drying is staged drying, first drying at room temperature for 40-50 h, and then drying at 45-55° C. for 45-55 h.
[0026] Furthermore, in step 3), the modified two-dimensional MXene material is obtained by modifying the two-dimensional MXene material with a natural phenolic compound;
[0027] The natural phenolic compounds include tannic acid.
[0028] The invention provides a room temperature self-repairing waterborne polyurethane film.
[0029] The present invention also provides an application of a room temperature self-repairing waterborne polyurethane film in a wearable device.
[0030] Beneficial effects of the present invention:
[0031] The waterborne polyurethane of the present invention has a gradient hydrogen bond network composed of single hydrogen bonds, double hydrogen bonds, quadruple hydrogen bonds and sextuple hydrogen bonds. By adjusting the ratio of different hydrogen bonds, the rigidity of the overall network and the fluidity of the waterborne polyurethane chain segments can be conveniently adjusted, so as to better selectively adjust the required performance. The self-healing waterborne polyurethane film provided by the present invention can achieve rapid self-healing at room temperature, and can also be applied to wearable sports sensors, and can maintain excellent sensing performance after being soaked in sweat.
[0032] The present invention can regulate the density of hydrogen bonds formed between waterborne polyurethane molecular chains by controlling the ratio of chain extenders and two-dimensional materials, and the multiple hydrogen bond networks provide waterborne polyurethane with excellent mechanical strength and toughness. Hydrogen bonds are typical dynamic non-covalent bonds, and the low bond energy enables waterborne polyurethane to achieve rapid self-repair at room temperature without heating. The waterborne polyurethane film of the present invention also has good water resistance, and can maintain good mechanical properties and self-repairing ability when exposed to water. Samples with added two-dimensional materials can also achieve rapid surface scratch self-repair under the induction of near-infrared light.
[0033] The synthesis method of the invention is simple, has low raw material cost, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The synthetic route of WPU-ADH3 in Comparative Example 4 is shown in FIG.
[0035] Figure 2 The stress-strain curve of the room temperature self-healing waterborne polyurethane film obtained in Example 1;
[0036] Figure 3The stress-strain curves of the room temperature self-healing waterborne polyurethane film obtained in Example 1 at different repair times;
[0037] Figure 4 The waterborne polyurethane film (WPU) obtained in Comparative Example 5, the self-healing waterborne polyurethane film (WPU-ADH3) obtained in Comparative Example 4, and the room temperature self-healing waterborne polyurethane film (WPU-ADH3-M) obtained in Example 1 were obtained. 0.5 )’s water resistance performance diagram;
[0038] Figure 5 WPU-ADH3-M after being soaked in sweat during exercise 0.5 Illustration of motion sensing using wearable flexible sensing materials. DETAILED DESCRIPTION
[0039] The present invention provides a method for preparing a room temperature self-repairing waterborne polyurethane film, comprising the following steps:
[0040] 1) mixing a polyether polyol and a chain extender, drying the mixture, and then adding a diisocyanate compound to carry out a polymerization reaction;
[0041] 2) adding a small molecule diol chain extender to the reaction system in step 1) to continue the reaction, and using an organic solvent to adjust the viscosity of the system;
[0042] 3) adding an amine compound to the reaction system of step 2) for neutralization reaction, and then adding a multi-hydrogen bond chain extender for dispersion to obtain a dispersion;
[0043] 4) The dispersion obtained in step 3) is subjected to rotary evaporation and then mixed with the modified two-dimensional MXene material, and the obtained mixture is placed in a mold and dried to obtain a room temperature self-healing waterborne polyurethane film.
[0044] In the present invention, the purpose of drying in step 1) is to remove moisture from the system.
[0045] In the present invention, in step 4), the dispersion is subjected to rotary evaporation to remove anhydrous butanone to obtain a self-healing waterborne polyurethane dispersion.
[0046] In the present invention, the mass ratio of the polyether polyol, the chain extender and the diisocyanate compound is 8-12:1:5-7, preferably 9-11:1:6, and more preferably 10:1:6;
[0047] The mass ratio of the chain extender, the small molecule diol chain extender and the amine compound is 1:0.7-1.2:0.6-1, preferably 1:0.8-1:0.7-0.9, and more preferably 1:0.9:0.8;
[0048] The mass ratio of the chain extender, the multiple hydrogen bond chain extender and the modified two-dimensional MXene material is 1:0.4-0.8:0.001-0.03, preferably 1:0.5-0.7:0.01-0.02, and more preferably 1:0.6:0.015.
[0049] In the present invention, in step 1), the polyether polyol comprises polypropylene glycol 2000 and / or polytetrahydrofuran diol, preferably polypropylene glycol 2000 or polytetrahydrofuran diol, and further preferably polypropylene glycol 2000;
[0050] The chain extender includes 2,2-dimethylol propionic acid and / or 2,2-dimethylol butyric acid, preferably 2,2-dimethylol propionic acid or 2,2-dimethylol butyric acid, and more preferably 2,2-dimethylol propionic acid;
[0051] The diisocyanate compound includes isophorone diisocyanate and / or hexamethylene diisocyanate, preferably isophorone diisocyanate or hexamethylene diisocyanate, and more preferably isophorone diisocyanate.
[0052] In the present invention, in step 1), the drying temperature is 100 to 130° C., preferably 120° C., and the drying time is 1.5 to 3 hours, preferably 1.8 to 2.5 hours, and more preferably 2 hours;
[0053] The polymerization reaction temperature is 82-100°C, preferably 85-95°C, more preferably 90°C, and the polymerization reaction time is 2.5-4h, preferably 2.8-3.5h, more preferably 3h;
[0054] The small molecule diol chain extender includes 1,4-butanediol, preferably 1,4-butanediol, and the organic solvent includes anhydrous butanone, preferably anhydrous butanone;
[0055] The reaction temperature is 70 to 80°C, preferably 72 to 78°C, more preferably 75°C, and the reaction time is 2 to 5 hours, preferably 2.5 to 4.5 hours, more preferably 3 hours;
[0056] The viscosity of the system is in the range of 30 to 60 mPa / s -1 , preferably 40 to 50 mPa / s -1 , more preferably 45mPa / s -1 .
[0057] In the present invention, in step 3), the amine compound includes triethylamine, preferably triethylamine;
[0058] The neutralization reaction temperature is 30-40°C, preferably 32-38°C, more preferably 35°C, and the neutralization reaction time is 20-40min, preferably 25-35°C, more preferably 28-32°C, more preferably 30°C;
[0059] The multiple hydrogen bond chain extender includes adipic acid dihydrazide and / or N,N-bis(2-hydroxyethyl)oxalamide, preferably adipic acid dihydrazide or N,N-bis(2-hydroxyethyl)oxalamide, and more preferably adipic acid dihydrazide.
[0060] In the present invention, in step 3), the dispersion rotation speed is 700-1000 rpm, preferably 750-950 rpm, more preferably 800-900 rpm, more preferably 850 rpm, and the dispersion time is 0.5-2 h, preferably 0.8-1.5 h, more preferably 1-1.3 h, more preferably 1.2 h.
[0061] In the present invention, in step 3), the mixing temperature is 20-40°C, preferably 25-35°C, and more preferably 30°C, and the mixing time is 0.5-2h, preferably 0.8-1.5h, and more preferably 1h; the drying is staged drying, first drying at room temperature for 40-50h, then drying at 45-55°C for 45-55h, preferably drying at room temperature for 42-48h, then drying at 48-52°C for 48-52h, more preferably drying at room temperature for 45h, and then drying at 50°C for 50h.
[0062] In the present invention, in step 3), the modified two-dimensional MXene material is obtained by modifying the two-dimensional MXene material with a natural phenolic compound;
[0063] The natural phenolic compounds include tannic acid, preferably tannic acid.
[0064] The invention provides a room temperature self-repairing waterborne polyurethane film.
[0065] The present invention also provides an application of a room temperature self-repairing waterborne polyurethane film in a wearable device.
[0066] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0067] Example 1
[0068] 31.2 g of polypropylene glycol 2000 and 3.485 g of 2,2-dimethylol propionic acid were added to a dry four-necked flask, vacuum dried at 110 ° C for 2 h, then cooled to 85 ° C, 20.17 g of isophorone diisocyanate was slowly added dropwise to carry out polymerization reaction for 3 h; then cooled to 75 ° C, 3.065 g of 1,4-butanediol was added dropwise to the reaction system to react for 2 h, and anhydrous butanone was used to adjust the system viscosity to 35 mPa / s -1 ; Continue to cool to 35°C, add 2.63 g of triethylamine to neutralize 2,2-dihydroxymethylpropionic acid, and react for 30 minutes.
[0069] 1.503 g of adipic acid dihydrazide was dissolved in deionized water, and the obtained adipic acid dihydrazide solution was added to the above reaction system, and then dispersed at a speed of 800 rpm for 1 hour. The obtained dispersion was rotary evaporated to remove anhydrous butanone to obtain a self-healing waterborne polyurethane dispersion, which was recorded as WPU-ADH3; the obtained self-healing waterborne polyurethane dispersion was then mixed with 0.0135 g of tannic acid-modified two-dimensional material MXene, stirred at 25°C for 1 hour, and then the obtained dispersion was poured into a polytetrafluoroethylene mold and dried at room temperature for 48 hours, and then dried at 50°C for 48 hours to obtain a room temperature self-healing waterborne polyurethane film, which was recorded as WPU-ADH3-M. 0.5 .
[0070] Example 2
[0071] 31.2 g of polytetrahydrofuran diol and 3.485 g of 2,2-dihydroxymethylbutyric acid were added to a dry four-necked flask, vacuum dried at 100 ° C for 3 h, then cooled to 82 ° C, and 20.17 g of hexamethylene diisocyanate was slowly added dropwise to carry out a polymerization reaction for 4 h; then cooled to 70 ° C, 3.065 g of 1,4-butanediol was added dropwise to the reaction system to react for 2 h, and anhydrous butanone was used to adjust the system viscosity to 40 mPa / s -1 ; Continue to cool to 30°C, add 2.63 g of triethylamine and 2,2-dihydroxymethylbutyric acid to neutralize 2,2-dihydroxymethylpropionic acid, and react for 40 minutes.
[0072] 1.503 g of N,N-bis(2-hydroxyethyl)oxalamide was dissolved in deionized water, the obtained N,N-bis(2-hydroxyethyl)oxalamide solution was added to the above reaction system, and then dispersed at 700 rpm for 2 hours. The obtained dispersion was rotary evaporated to remove anhydrous butanone to obtain a self-healing waterborne polyurethane dispersion; the obtained self-healing waterborne polyurethane dispersion was mixed with 0.0135 g of tannic acid-modified two-dimensional material MXene, stirred at 20°C for 2 hours, and the obtained dispersion was poured into a polytetrafluoroethylene mold and dried at room temperature for 50 hours, and then dried at 45°C for 45 hours to obtain a room temperature self-healing waterborne polyurethane film, recorded as WPU-BHO2-M1.
[0073] Example 3
[0074] 31.2 g of polypropylene glycol 2000 and 3.485 g of 2,2-dihydroxymethylbutyric acid were added to a dry four-necked flask, vacuum dried at 130 ° C for 1.5 h, then cooled to 100 ° C, and 20.17 g of hexamethylene diisocyanate was slowly added dropwise to carry out polymerization reaction for 2.5 h; then cooled to 80 ° C, 3.065 g of 1,4-butanediol was added dropwise to the reaction system to react for 5 h, and anhydrous butanone was used to adjust the system viscosity to 32 mPa / s -1 ; Continue to cool to 40°C, add 2.63 g of triethylamine to neutralize 2,2-dihydroxymethylpropionic acid, and react for 20 minutes.
[0075] 2.247 g of N,N-bis(2-hydroxyethyl)oxamide and 2.123 g of adipic acid dihydrazide were dissolved in deionized water, the resulting solution was added to the above reaction system, and then dispersed at a speed of 1000 rpm for 0.5 h. The obtained dispersion was rotary evaporated to remove anhydrous butanone to obtain a self-healing waterborne polyurethane dispersion; the obtained self-healing waterborne polyurethane dispersion was stirred with 0.0135 g of tannic acid-modified two-dimensional material MXene at 40 °C for 0.5 h, the obtained dispersion was poured into a polytetrafluoroethylene mold and dried at room temperature for 40 h, and then dried at 55 °C for 55 h to obtain a room temperature self-healing waterborne polyurethane film, recorded as WPU-BHO2 / ADH3-M1.
[0076] Comparative Example 4
[0077] Different from Example 1, in this comparative example, tannic acid-modified two-dimensional material MXene is not added, and the self-healing waterborne polyurethane dispersion is directly poured into a polytetrafluoroethylene mold and dried at room temperature for 48 hours, and then dried at 50°C for 48 hours to obtain a room temperature self-healing waterborne polyurethane film, which is recorded as WPU-ADH3.
[0078] Comparative Example 5
[0079] 31.2 g of polypropylene glycol 2000 and 3.485 g of 2,2-dimethylol propionic acid were added to a dry four-necked flask, vacuum dried at 110 ° C for 2 h, then cooled to 85 ° C, 20.17 g of isophorone diisocyanate was slowly added dropwise to carry out polymerization reaction for 3 h; then cooled to 75 ° C, 3.065 g of 1,4-butanediol was added dropwise to the reaction system to react for 2 h, and anhydrous butanone was used to adjust the system viscosity to 35 mPa / s -1 ; Continue to cool to 35°C, add 2.63g of triethylamine to neutralize 2,2-dihydroxymethyl propionic acid, and react for 30 minutes. After adding deionized water, disperse at a speed of 800rpm to obtain the desired WPU.
[0080] It can be seen from the above embodiments that the present invention provides a room temperature self-healing waterborne polyurethane film and a preparation method and application thereof. Figure 2 is the stress-strain curve of the room temperature self-healing waterborne polyurethane film obtained in Example 1, Figure 2 It can be seen that the room temperature self-healing waterborne polyurethane film of the present invention has good mechanical properties; Figure 3 The stress-strain curves of the room temperature self-healing waterborne polyurethane film obtained in Example 1 at different repair times are shown in FIG. Figure 3 It can be seen that the room temperature self-healing waterborne polyurethane film of the present invention has good self-healing performance; the samples were placed in water and the appearance of the samples was observed after absorbing water for 24 hours. Figure 4 The waterborne polyurethane film (WPU) obtained in comparative example 5, the self-healing waterborne polyurethane film (WPU-ADH3) obtained in comparative example 4, and the room temperature self-healing waterborne polyurethane film (WPU-ADH3-M) obtained in example 1 are respectively 0.5 ) water resistance performance diagram. It can be seen from the figure that after absorbing water for 24 hours, WPU showed structural collapse, while WPU-ADH3 and WPU-ADH3-M 0.5 The structure of the WPU-ADH3-M obtained in Example 1 is intact, which proves that the material has significantly enhanced water resistance. 0.5 As a flexible sensing material, it is used to monitor human motion. The material is worn on the elbow joint and connected to the electrochemical workstation to monitor WPU-ADH3-M 0.5 The resistance change of the elbow can be observed at different bending angles. Figure 5 WPU-ADH3-M after being soaked in sweat during exercise 0.5 The motion sensing diagram of the material shows that when the room temperature self-healing waterborne polyurethane film of the present invention is applied to wearable devices, it can not only monitor and distinguish different motion states of the human body very conveniently, but also maintain excellent sensing performance after being soaked in sweat. It can be seen that the self-healing waterborne polyurethane film prepared by the self-healing waterborne polyurethane dispersion based on multiple gradient hydrogen bonds of the present invention has excellent mechanical strength and toughness, and has rapid room temperature self-healing ability. Due to the tightly bound network, the waterborne polyurethane also has significantly enhanced water resistance, and has good application prospects in multifunctional self-healing waterborne polyurethane.
[0081] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a room temperature self-repairing waterborne polyurethane film, characterized in that: The following steps are involved: 1) mixing a polyether polyol and a chain extender, drying the mixture, and then adding a diisocyanate compound to carry out a polymerization reaction; 2) adding a small molecule diol chain extender to the reaction system in step 1) to continue the reaction, and using an organic solvent to adjust the viscosity of the system; 3) adding an amine compound to the reaction system of step 2) for neutralization reaction, and then adding a multi-hydrogen bond chain extender for dispersion to obtain a dispersion; 4) The dispersion obtained in step 3) is subjected to rotary evaporation and then mixed with the modified two-dimensional MXene material, and the obtained mixture is placed in a mold and dried to obtain a room temperature self-healing waterborne polyurethane film.
2. The method for preparing a room temperature self-repairing waterborne polyurethane film according to claim 1, characterized in that: The mass ratio of the polyether polyol, the chain extender and the diisocyanate compound is 8-12:1:5-7; The mass ratio of the chain extender, the small molecule diol chain extender and the amine compound is 1:0.7-1.2:0.6-1; The mass ratio of the chain extender, the multiple hydrogen bond chain extender and the modified two-dimensional MXene material is 1:0.4~0.8:0.001~0.
03.
3. The method for preparing a room temperature self-repairing waterborne polyurethane film according to claim 1, characterized in that: In step 1), the polyether polyol comprises polypropylene glycol 2000 and / or polytetrahydrofuran diol; The chain extender includes 2,2-dimethylol propionic acid and / or 2,2-dimethylol butyric acid; The diisocyanate compound includes isophorone diisocyanate and / or hexamethylene diisocyanate.
4. The method for preparing a room temperature self-repairing waterborne polyurethane film according to claim 1 or 3, characterized in that: In step 1), the drying temperature is 100-130° C. and the drying time is 1.5-3 hours; The polymerization reaction temperature is 82-100° C., and the polymerization reaction time is 2.5-4 hours; The small molecule diol chain extender includes 1,4-butanediol, and the organic solvent includes anhydrous butanone; The reaction temperature is 70-80°C and the reaction time is 2-5h; The viscosity of the system is in the range of 30 to 60 mPa / s -1 .
5. The method for preparing a room temperature self-repairing waterborne polyurethane film according to claim 4, characterized in that: In step 3), the amine compound includes triethylamine; The neutralization reaction temperature is 30-40°C, and the neutralization reaction time is 20-40 minutes; The multiple hydrogen bond chain extender includes adipic acid dihydrazide and / or N,N-bis(2-hydroxyethyl)oxalamide.
6. The method for preparing a room temperature self-repairing waterborne polyurethane film according to claim 5, characterized in that: In step 3), the dispersion speed is 700-1000 rpm, and the dispersion time is 0.5-2 h.
7. The method for preparing a room temperature self-repairing waterborne polyurethane film according to claim 6, characterized in that: In step 3), the mixing temperature is 20-40° C., and the mixing time is 0.5-2 h; the drying is staged drying, first drying at room temperature for 40-50 h, and then drying at 45-55° C. for 45-55 h.
8. The method for preparing a room temperature self-repairing waterborne polyurethane film according to claim 6 or 7, characterized in that: In step 3), the modified two-dimensional MXene material is obtained by modifying the two-dimensional MXene material with a natural phenolic compound; The natural phenolic compounds include tannic acid.
9. A room temperature self-healing waterborne polyurethane film prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the room temperature self-healing waterborne polyurethane film according to claim 9 in wearable devices.
Citation Information
Patent Citations
Self-repairing waterborne polyurethane film and preparation method thereof
CN116355249A
Preparation method and application of flexible self-supporting MXene / plant polyphenol composite film electrode
CN116469696A
Antibacterial and self-repairing composite coating based on visible light induction MXene / waterborne polyurethane and preparation method of antibacterial and self-repairing composite coating
CN116694219A
Self-repairable elastomer applied to optical driver and preparation method of self-repairable elastomer
CN117659678A
Enhanced, self-healable or recoverable and recyclable 3D printed article and preparation method and use thereof
US20220315673A1
Cited By
Modified intelligent wearable TPU (thermoplastic polyurethane) capable of improving self-repairing capability and preparation method of modified intelligent wearable TPU
CN120944065A