High-temperature hydrophobic aerogel composite material and preparation method thereof
By adding high-temperature resistant aerogel and modified vermiculite to the aerogel composite material, combined with functional addition of components, the performance degradation of aerogel composite material in humid and high-temperature environments is solved, and its insulation is achieved Widely used and long-term use in the field of thermal insulation.
Patent Information
- Application Number
- CN202411278902.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-12
AI Technical Summary
Aerogel composites are prone to adsorbing water vapor in humid environments, resulting in increased thermal conductivity, decreased thermal insulation performance, and are unstable in high-temperature environments, making it difficult to suppress oxidation and affect their service life.
A high-temperature hydrophobic aerogel composite material is prepared, including hydrolysis in ethyl orthosilicate and adding mullite fibers to form a high-temperature resistant aerogel, and reacting with an epoxy modifier by activating vermiculite , graft caffeic acid, prepare composite additives, combine functional additives to form an aerogel composite material with antioxidant and hydrophobic properties.
It significantly improves the high temperature resistance, thermal insulation, hydrophobicity and oxidation resistance of aerogel composites, extends its service life, and ensures stability and performance in high temperature and humid and heat environments.
Smart Images

Figure CN118909402A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a high-temperature hydrophobic aerogel composite material and a preparation method thereof. Background Art
[0002] With the continuous development of science and technology, the application of aerogel composites is increasing. Aerogel composites are a new type of material that has both the characteristics of aerogel and the advantages of other materials. Aerogel composites are divided into inorganic aerogels, organic aerogels and organic-inorganic aerogels. It is a lightweight material with a nanoporous network structure and the network pores are filled with gaseous dispersion medium. It has many advantages such as ultra-low density, high specific surface area, high porosity, low light refractive index, sound insulation, etc. The high specific surface area and high porosity make aerogel composites have extremely low thermal conductivity, and it has great application potential in the field of thermal insulation.
[0003] Epoxy resin has excellent processing performance and dielectric properties, and is widely used in insulation, electronic and electrical industries. Aerogel itself is an excellent thermal insulation material. Adding aerogel to epoxy resin to prepare aerogel composites can improve the thermal insulation properties of the epoxy resin matrix. However, due to the porous structure of aerogel composites, it is easy to adsorb water vapor in a humid environment, resulting in increased thermal conductivity and decreased thermal insulation properties. At the same time, in order to make the aerogel composites maintain stable performance in high temperature environments, and inhibit or slow down the effects of oxidation in humid and hot environments, it is necessary to modify the aerogel composites so that the aerogel composites have low thermal conductivity, excellent high temperature resistance, hydrophobicity, antioxidant properties and mechanical properties to meet the thermal insulation needs in various environments.
[0004] Patent publication number CN113512272B discloses a method for preparing a low thermal conductivity aerogel epoxy resin thermal insulation composite material. The composite material is prepared by mixing aerogel particles with epoxy resin, exhausting bubbles using negative pressure, and centrifuging the mixture at different gradient speeds to improve the curing strength of the composite material. The prepared aerogel epoxy resin thermal insulation composite material has low thermal conductivity and improved thermal insulation performance. However, the patent does not take into account the effects of oxidation on the aerogel composite material in a hot and humid environment and the application of hydrophobic aerogel composite materials. Therefore, the present invention provides a high-temperature hydrophobic aerogel composite material with a long service life and broad application prospects. Summary of the invention
[0005] In order to solve the problems mentioned in the background technology, the object of the present invention is to provide a high-temperature hydrophobic aerogel composite material and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions: A high-temperature hydrophobic aerogel composite material comprises the following raw materials in parts by weight: 70-90 parts of epoxy resin, 40-60 parts of diluent, 10-15 parts of curing agent, 1-3 parts of anti-ultraviolet additive, 1-3 parts of flame retardant additive, 5-8 parts of high-temperature resistant aerogel, 3-6 parts of composite additives, and 4-6 parts of functional additive components.
[0007] Furthermore, the method for preparing the high temperature resistant aerogel comprises the following steps: S1. Add deionized water and ethanol to tetraethyl orthosilicate, stir and mix evenly, add hydrochloric acid to adjust the pH to 3-4, and hydrolyze for 4-6 hours to obtain an aerogel hydrolyzate; S2. Add mullite fiber to the aerogel hydrolyzate and disperse it evenly, then add dilute ammonia water to adjust the pH to 6-8. After 1-2 hours, gel is formed. The gel is placed in anhydrous ethanol at room temperature for aging for 12-18 hours, and finally dried at 45-65°C to obtain high temperature resistant aerogel.
[0008] By adopting the above technical scheme, tetraethyl orthosilicate can be hydrolyzed under acidic conditions to obtain an aerogel hydrolyzate, and after adding mullite fibers with excellent chemical stability and high temperature resistance, gelation, aging and drying are carried out under alkaline conditions to obtain a high temperature resistant aerogel. The mullite fibers are overlapped into a network internally, so that the prepared high temperature resistant aerogel has excellent mechanical strength, a stable internal structure, and is not easy to collapse. When added to an epoxy resin matrix, the high temperature resistance of the aerogel composite material can be significantly improved.
[0009] Furthermore, in step S2, the mass percentage of the mullite fiber in the aerogel hydrolyzate is 6-8%.
[0010] Furthermore, the preparation method of the composite additive comprises the following steps: Step A, adding activated vermiculite to a sodium hydroxide solution with a mass fraction of 6-8% and dispersing the mixture evenly, adding an epoxy modifier, and then placing the mixture in a water bath and raising the temperature to 60-70° C., reacting for 3-5 hours, cooling, washing, filtering, and vacuum drying to obtain modified vermiculite; Step B, adding modified vermiculite into dimethyl sulfoxide and dispersing it evenly, then adding caffeic acid and p-toluenesulfonic acid, and then raising the temperature to 85-95° C., reacting for 4-6 hours, centrifuging, washing, and vacuum drying to obtain a composite additive.
[0011] By adopting the above technical scheme, after the vermiculite is treated with hydrochloric acid, the active silanol groups can be exposed. Under alkaline conditions, the silanol groups in the activated vermiculite can undergo a ring-opening reaction with the epoxy groups in the epoxy modifier to obtain modified vermiculite with active hydroxyl groups. Under the action of p-toluenesulfonic acid, the active hydroxyl groups in the modified vermiculite undergo an esterification reaction with the active carboxyl groups in the caffeic acid structure, thereby grafting caffeic acid with antioxidant effect on the surface of the vermiculite to obtain a composite additive.
[0012] Furthermore, in step A, the method for activating vermiculite is to mix the vermiculite with a hydrochloric acid solution having a mass fraction of 6-8%, stir for 1-2 hours in a water bath at 70-80°C, wash to neutrality, and dry at 50-60°C to obtain activated vermiculite.
[0013] Furthermore, in step A, the epoxy modifier is any one of 1,2-epoxydodecane, 1,2-epoxytetradecane, 1,2-epoxyhexadecane or 1,2-epoxyoctadecane.
[0014] Furthermore, the preparation method of the functional additive component is as follows: Ⅰ. Add polyisoprene to toluene, stir evenly, introduce nitrogen protection, then add mercaptoethylamine and benzoin dimethyl ether, and react under ultraviolet light for 2-3 hours. After the reaction is completed, wash and vacuum dry to obtain modified polyisoprene; Ⅱ. Add modified polyisoprene to N,N-dimethylformamide, stir evenly, introduce nitrogen protection, then add 3-bromopropyl tert-butyl dimethylsilyl ether and alkaline catalyst, raise the temperature to 60-80°C, react for 4-6h, cool to room temperature, wash, and vacuum dry to obtain functional additive components.
[0015] By adopting the above technical scheme, the alkenyl group in the polyisoprene structure can undergo a click reaction with the active thiol group in the mercaptoethylamine structure under the irradiation of benzoin dimethyl ether and ultraviolet light, thereby introducing an active amino group into the polyisoprene to obtain modified polyisoprene. The active amino group in the modified polyisoprene structure can undergo a substitution reaction with the active bromine substituent in the 3-bromopropyl tert-butyl dimethylsilyl ether structure under the action of an alkaline catalyst to obtain a functional additive component.
[0016] Furthermore, in step II, the alkaline catalyst is triethylamine or pyridine.
[0017] Furthermore, the diluent is acetone or xylene; the curing agent is methyltetrahydrophthalic anhydride or methylhexahydrophthalic anhydride; the anti-ultraviolet additive is UV-1577 or UV-327; and the flame retardant additive is dimethyl methyl phosphate or toluene diphenyl phosphate.
[0018] A method for preparing a high-temperature hydrophobic aerogel composite material comprises the following steps: Step 1: Add epoxy resin, diluent, anti-ultraviolet additive, flame retardant additive, high temperature resistant aerogel, composite additive and functional additive component into a mixing tank and mix them evenly. Centrifuge the mixture at 1000-2000 r / min for 3-5 minutes to obtain a mixture. Step 2: Add the curing agent to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 20-40 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold, cure it at 160-200° C. for 3-5 hours, and after curing, naturally cool and demould to obtain an aerogel composite material.
[0019] Beneficial effects of the present invention: (1) The high temperature resistant aerogel prepared by the present invention is added to the epoxy resin matrix to form a heat insulation barrier, which limits heat transfer and can significantly improve the high temperature resistance and thermal insulation performance of the aerogel composite material. As a result, the aerogel composite material can still have stability, reliability and low thermal conductivity in a high temperature environment, thereby broadening the application scope of the aerogel composite material in the field of thermal insulation.
[0020] (2) The composite additive prepared by the present invention grafts caffeic acid with antioxidant effect onto the surface of vermiculite. On the one hand, after the vermiculite is grafted and modified, the compatibility between the vermiculite and the epoxy resin matrix is effectively improved, and the agglomeration of the vermiculite in the matrix is avoided. The vermiculite can be evenly distributed in the epoxy resin matrix, thereby improving the binding force between the vermiculite and the epoxy resin matrix, giving full play to the advantages of the vermiculite, and improving the mechanical properties of the epoxy resin matrix. At the same time, the vermiculite has a lamellar structure and is evenly dispersed in the epoxy resin matrix to form a physical barrier layer, which can block the infiltration of water vapor and has a synergistic hydrophobic effect with the functional additive component. On the other hand, after the caffeic acid is grafted onto the vermiculite, the small molecule caffeic acid is not easy to migrate, so that the prepared composite additive has excellent antioxidant properties. When added to the epoxy resin matrix, it has long-lasting antioxidant properties, thereby preventing the aerogel composite material from being oxidized in a hot and humid environment, thereby extending the service life of the aerogel composite material.
[0021] (3) The functional additive component prepared by the present invention contains secondary amino groups, which can be cross-linked with the epoxy resin molecular chain to increase the cross-linking density, enhance the compactness of the aerogel composite material structure, reduce the molecular gap, and prevent water penetration. In addition, the functional additive component contains hydrophobic siloxane and a strongly hydrophobic tert-butyl structure, which exhibits extremely low surface energy, can make the aerogel composite material more hydrophobic, and further prevent water molecules from penetrating and invading. In addition, the siloxane in the functional additive component has a high bond energy and can be cross-linked with the epoxy resin matrix, which can enhance the high temperature resistance of the aerogel composite material to a certain extent, and has a synergistic effect with the high temperature resistant aerogel.
[0022] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0024] Figure 1 The infrared spectra of activated vermiculite, modified vermiculite and composite additives in the embodiments of the present invention are shown in FIG. Figure 2 This is an infrared spectrum of the functional added component in the embodiment of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] Preparation of high temperature resistant aerogel S1. Add 20 mL of deionized water and 40 mL of ethanol to 8 mL of ethyl orthosilicate, stir and mix evenly, then add hydrochloric acid to adjust the pH to 3.5, and hydrolyze for 6 hours to obtain an aerogel hydrolyzate; S2. Add 0.6 g of mullite fiber to 10 mL of aerogel hydrolyzate and disperse it evenly. Then add dilute ammonia water to adjust the pH to 7. After 2 hours, gel is formed. The gel is placed in anhydrous ethanol at room temperature for aging for 16 hours. Finally, it is dried at 60°C to obtain high temperature resistant aerogel.
[0028] Example 2
[0029] Preparation of composite additives Step A, 3.5 g of vermiculite was mixed with 8% hydrochloric acid solution by mass, stirred for 2 h in a 75° C. water bath, washed until neutral, and dried at 60° C. to obtain activated vermiculite; Step B, adding 3.2g of activated vermiculite to a 7% sodium hydroxide solution and dispersing the mixture evenly, adding 2.8g of 1,2-epoxyhexadecane, and then placing the mixture in a water bath and raising the temperature to 60°C. After reacting for 4h, the mixture was cooled, washed, filtered, and vacuum dried to obtain modified vermiculite; Step C, adding 2.8g of modified vermiculite into dimethyl sulfoxide and dispersing it evenly, then adding 2.3g of caffeic acid and 0.3g of p-toluenesulfonic acid, and then raising the temperature to 95°C, reacting for 5h, centrifuging, washing, and vacuum drying to obtain a composite additive.
[0030] The activated vermiculite, modified vermiculite and composite additives were tested by Fourier transform infrared spectrometer. Figure 1 As shown, the spectral wavenumber test range is 4000cm -1 -500cm -1 , analysis shows that in the infrared spectrum of activated vermiculite, 3408cm -1 The absorption peak of hydroxyl group appeared at 1015cm -1 There is a Si-O absorption peak at 689 cm -1 The absorption peak of Al-O-Si appears at 2960cm -1 -2865cm -1 The absorption peaks of methylene and methyl appeared at 1030 cm -1 The absorption peak area of Si-O increases; in the infrared spectrum of the composite additive, 3069cm -1 The absorption peak of CH in the carbon-carbon double bond appears at 3026 cm -1 The absorption peak of CH in the benzene ring appeared at 1730 cm -1 The absorption peak of C=O in the ester group appeared.
[0031] Example 3
[0032] Preparation of functional additives Ⅰ. Add 3g of polyisoprene to toluene, stir evenly, introduce nitrogen protection, then add 2.5g of mercaptoethylamine and 0.3g of benzoin dimethyl ether, and react under ultraviolet light for 2.5h. After the reaction is completed, wash and vacuum dry to obtain modified polyisoprene; Ⅱ. Add 2.6 g of modified polyisoprene to N,N-dimethylformamide, stir evenly, introduce nitrogen protection, then add 2 g of 3-bromopropyl tert-butyl dimethylsilyl ether and 0.4 g of triethylamine, raise the temperature to 70°C, react for 5 hours, cool to room temperature, wash, and vacuum dry to obtain a functional additive component.
[0033] The functional additive components were tested by Fourier infrared spectrometer, such as Figure 2 As shown, the spectral wavenumber test range is 4000cm -1 -500cm -1 , analysis shows that in the infrared spectrum of the functional additive component, 3414cm -1 The absorption peak of NH appeared at 2960-2850cm -1 The absorption peaks of methylene and methyl appeared at 1367 cm -1 The absorption peak of tert-butyl appeared at 1176 cm -1 The absorption peak of CSC appeared at 1032cm -1 The absorption peak of Si-OC appeared at 798 cm -1 The absorption peak of Si-C appears at
[0034] Example 4
[0035] Preparation of aerogel composites Step 1: add 70g of epoxy resin, 40g of acetone, 1g of anti-ultraviolet additive UV-327, 1g of flame retardant additive dimethyl methyl phosphate, 5g of the high temperature resistant aerogel prepared in Example 1, 3g of the composite additive prepared in Example 2, and 4g of the functional additive component prepared in Example 3 into a mixing tank and mix evenly, and centrifuge the mixture at 1000r / min for 3min to obtain a mixture; Step 2: Add 10 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 20 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 160° C. for 3 h. After curing, naturally cool and demould to obtain an aerogel composite material.
[0036] Example 5
[0037] Preparation of aerogel composites Step 1: 80 g of epoxy resin, 50 g of acetone, 2 g of anti-ultraviolet additive UV-327, 2 g of flame retardant additive dimethyl methyl phosphate, 6 g of the high temperature resistant aerogel prepared in Example 1, 5 g of the composite additive prepared in Example 2, and 5 g of the functional additive component prepared in Example 3 are added into a mixing tank and mixed evenly. The mixture is centrifuged at 1500 r / min for 4 min to obtain a mixture. Step 2: Add 12 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 30 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 180° C. for 4 h. After the curing is completed, the aerogel composite material is obtained after natural cooling and demoulding.
[0038] Example 6
[0039] Preparation of aerogel composites Step 1: 90 g of epoxy resin, 60 g of acetone, 3 g of anti-ultraviolet additive UV-327, 3 g of flame retardant additive dimethyl methyl phosphate, 8 g of the high temperature resistant aerogel prepared in Example 1, 6 g of the composite additive prepared in Example 2, and 6 g of the functional additive component prepared in Example 3 are added into a mixing tank and mixed evenly. The mixture is centrifuged at 2000 r / min for 5 min to obtain a mixture. Step 2: Add 15 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 40 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 200° C. for 5 h. After the curing is completed, the aerogel composite material is obtained after natural cooling and demoulding.
[0040] Comparative Example 1 Preparation of aerogel composites Step 1: 80 g of epoxy resin, 50 g of acetone, 2 g of anti-ultraviolet additive UV-327, 2 g of flame retardant additive dimethyl methyl phosphate, 5 g of the composite additive prepared in Example 2, and 5 g of the functional additive component prepared in Example 3 are added into a mixing tank and mixed evenly. The mixture is centrifuged at 1500 r / min for 4 min to obtain a mixture. Step 2: Add 12 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 30 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 180° C. for 4 h. After the curing is completed, the aerogel composite material is obtained after natural cooling and demoulding.
[0041] Comparative Example 2 Preparation of aerogel composites Step 1: 80 g of epoxy resin, 50 g of acetone, 2 g of anti-ultraviolet additive UV-327, 2 g of flame retardant additive dimethyl methyl phosphate, 6 g of the high temperature resistant aerogel prepared in Example 1, and 5 g of the functional additive component prepared in Example 3 were added into a mixing tank and mixed evenly. The mixture was centrifuged at 1500 r / min for 4 min to obtain a mixture. Step 2: Add 12 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 30 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 180° C. for 4 h. After the curing is completed, the aerogel composite material is obtained after natural cooling and demoulding.
[0042] Comparative Example 3 Preparation of aerogel composites Step 1, add 80g of epoxy resin, 50g of acetone, 2g of anti-ultraviolet additive UV-327, 2g of flame retardant additive dimethyl methyl phosphate, 6g of the high temperature resistant aerogel prepared in Example 1, and 5g of the composite additive prepared in Example 2 into a mixing tank and mix them evenly, and centrifuge the mixture at 1500r / min for 4min to obtain a mixture; Step 2: Add 12 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 30 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 180° C. for 4 h. After the curing is completed, the aerogel composite material is obtained after natural cooling and demoulding.
[0043] Comparative Example 4 Preparation of aerogel composites Step 1: 80 g of epoxy resin, 50 g of acetone, 2 g of anti-ultraviolet additive UV-327, 2 g of flame retardant additive dimethyl methyl phosphate, 6 g of the high temperature resistant aerogel prepared in Example 1, 5 g of vermiculite, and 5 g of the functional additive component prepared in Example 3 were added into a mixing tank and mixed evenly. The mixture was centrifuged at 1500 r / min for 4 min to obtain a mixture. Step 2: Add 12 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 30 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 180° C. for 4 h. After the curing is completed, the aerogel composite material is obtained after natural cooling and demoulding.
[0044] Comparative Example 5 Preparation of aerogel composites Step 1, 80g of epoxy resin, 50g of acetone, 2g of anti-ultraviolet additive UV-327, 2g of flame retardant additive dimethyl methyl phosphate, 6g of the high temperature resistant aerogel prepared in Example 1, 5g of the composite additive prepared in Example 2, and 5g of polyisoprene are added into a mixing tank and mixed evenly, and the mixture is centrifuged at 1500r / min for 4min to obtain a mixture; Step 2: Add 12 g of methyltetrahydrophthalic anhydride to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 30 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold and cure it at 180° C. for 4 h. After the curing is completed, the aerogel composite material is obtained after natural cooling and demoulding.
[0045] Performance Testing The performance of the aerogel composite materials prepared in Example 4 to Example 6 and Comparative Examples 1 to Comparative Examples 5 was tested. 5 mg of the aerogel composite material was weighed and placed in an oven. The temperature was increased from 25°C to 800°C at a heating rate of 10°C / min. The initial decomposition temperature of the aerogel composite material was recorded to determine the high temperature resistance of the aerogel composite material. According to the GB / T10295-2008 standard, the thermal conductivity of the aerogel composite material was tested to determine the thermal insulation performance of the aerogel composite material. According to the GB / T 10299-2011 standard, the hydrophobicity of the aerogel composite material was tested to determine the hydrophobic performance. According to GB / T 1040.2-2022, the tensile properties of the aerogel composite material were tested, and then the aerogel composite material was placed in an aging box at 250°C. After aging for 24 hours, the tensile properties of the aerogel composite material were tested again to determine the antioxidant properties and mechanical properties of the aerogel composite material. The test results are shown in the following table:
[0046] As can be seen from the above table, the aerogel composite materials prepared by Examples 4 to 6 of the present invention have excellent high temperature resistance, thermal insulation, hydrophobicity, oxidation resistance and mechanical properties, among which the test result of Example 5 is the best. Comparative Example 1 does not add high temperature resistant aerogel, and the high temperature resistance test and thermal insulation test results are poor; Comparative Example 2 does not add composite additives, and vermiculite grafted antioxidant small molecule caffeic acid cannot be used to improve the oxidation resistance, hydrophobicity and mechanical properties of the aerogel composite material, so the oxidation resistance test, hydrophobicity test and mechanical property test results are poor; Comparative Example 3 does not add functional additive components, and hydrophobic siloxane and strong hydrophobic tert-butyl structure cannot be used to improve the hydrophobicity of the aerogel composite material. And the functional added components are cross-linked with the epoxy resin matrix to improve the compactness of the aerogel composite material, and the high bond energy silicon-oxygen bonds improve the high temperature resistance, so the high temperature resistance test and the hydrophobicity test results are poor; in Comparative Example 4, vermiculite is added, and the vermiculite is directly added to the epoxy resin matrix without modification, which is prone to agglomeration, so the hydrophobicity test and the mechanical property test results are poor, and it is not grafted with caffeic acid with antioxidant effect, so the antioxidant performance test result is poor; in Comparative Example 5, polyisoprene is added, and the hydrophobicity cannot be improved by using the tert-butyl structure and siloxane with strong hydrophobicity, and the high bond energy silicon-oxygen bonds and cross-linking with the epoxy resin matrix, so the high temperature resistance test and the hydrophobicity test results are poor.
[0047] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A high temperature hydrophobic aerogel composite material, It is characterized in that The invention comprises the following raw materials in parts by weight: 70-90 parts of epoxy resin, 40-60 parts of diluent, 10-15 parts of curing agent, 1-3 parts of anti-ultraviolet additive, 1-3 parts of flame retardant additive, 5-8 parts of high temperature resistant aerogel, 3-6 parts of composite additive and 4-6 parts of functional additive component.
2. A high temperature hydrophobic aerogel composite material according to claim 1, It is characterized in that The method for preparing the high temperature resistant aerogel comprises the following steps: S1. Add deionized water and ethanol to tetraethyl orthosilicate, stir and mix evenly, add hydrochloric acid to adjust the pH to 3-4, and hydrolyze for 4-6 hours to obtain an aerogel hydrolyzate; S2. Add mullite fiber to the aerogel hydrolyzate and disperse it evenly, then add dilute ammonia water to adjust the pH to 6-8. After 1-2 hours, gel is formed. The gel is placed in anhydrous ethanol at room temperature for aging for 12-18 hours, and finally dried at 45-65°C to obtain high temperature resistant aerogel.
3. A high temperature hydrophobic aerogel composite material according to claim 2, It is characterized in that In step S2, the mass percentage of the mullite fiber in the aerogel hydrolyzate is 6-8%.
4. The high temperature hydrophobic aerogel composite material according to claim 1, It is characterized in that The preparation method of the composite additive comprises the following steps: Step A, adding activated vermiculite to a sodium hydroxide solution with a mass fraction of 6-8% and dispersing the mixture evenly, adding an epoxy modifier, and then placing the mixture in a water bath and raising the temperature to 60-70° C., reacting for 3-5 hours, cooling, washing, filtering, and vacuum drying to obtain modified vermiculite; Step B, adding modified vermiculite into dimethyl sulfoxide and dispersing it evenly, then adding caffeic acid and p-toluenesulfonic acid, and then raising the temperature to 85-95° C., reacting for 4-6 hours, centrifuging, washing, and vacuum drying to obtain a composite additive.
5. A high temperature hydrophobic aerogel composite material according to claim 4, It is characterized in that In step A, the method for activating vermiculite is to mix the vermiculite with a hydrochloric acid solution with a mass fraction of 6-8%, stir for 1-2 hours in a water bath at 70-80° C., wash to neutrality, and dry at 50-60° C. to obtain activated vermiculite.
6. A high temperature hydrophobic aerogel composite material according to claim 4, It is characterized in that In step A, the epoxy modifier is any one of 1,2-epoxydodecane, 1,2-epoxytetradecane, 1,2-epoxyhexadecane or 1,2-epoxyoctadecane.
7. The high temperature hydrophobic aerogel composite material according to claim 1, It is characterized in that The preparation method of the functional additive component comprises the following steps: Ⅰ. Add polyisoprene to toluene, stir evenly, introduce nitrogen protection, then add mercaptoethylamine and benzoin dimethyl ether, and react under ultraviolet light for 2-3 hours. After the reaction is completed, wash and vacuum dry to obtain modified polyisoprene; Ⅱ. Add modified polyisoprene to N,N-dimethylformamide, stir evenly, introduce nitrogen protection, then add 3-bromopropyl tert-butyl dimethylsilyl ether and alkaline catalyst, raise the temperature to 60-80°C, react for 4-6h, cool to room temperature, wash, and vacuum dry to obtain functional additive components.
8. A high temperature hydrophobic aerogel composite material according to claim 7, It is characterized in that In step II, the basic catalyst is triethylamine or pyridine.
9. The high temperature hydrophobic aerogel composite material according to claim 1, It is characterized in that The diluent is acetone or xylene; the curing agent is methyltetrahydrophthalic anhydride or methylhexahydrophthalic anhydride; the anti-ultraviolet additive is UV-1577 or UV-327; and the flame retardant additive is dimethyl methyl phosphate or toluene diphenyl phosphate.
10. A method for preparing the high temperature hydrophobic aerogel composite material as claimed in claim 1, It is characterized in that The following steps are involved: Step 1: Add epoxy resin, diluent, anti-ultraviolet additive, flame retardant additive, high temperature resistant aerogel, composite additive and functional additive component into a mixing tank and mix them evenly. Centrifuge the mixture at 1000-2000 r / min for 3-5 minutes to obtain a mixture. Step 2: Add the curing agent to the mixture, stir evenly, place in a vacuum drying oven and evacuate for 20-40 minutes to degas, and obtain a treated material; Step 3: pour the treated material into a mold, cure it at 160-200° C. for 3-5 hours, and after curing, naturally cool and demould to obtain an aerogel composite material.
Citation Information
Patent Citations
A method for preparing a low thermal conductivity aerogel-type epoxy resin thermal insulation composite material
CN113512272B
SiO2 aerogel flame-retardant epoxy resin composite material and preparation method thereof
CN110066495A
Combined energy absorption method and application thereof
CN111378138A
Preparation method of high-temperature-resistant aerogel composite material and composite material thereof
CN114804819A
Composite insulation board containing hybrid aerogel and preparation method thereof
CN118290904A
Cited By
Silica aerogel composite thermal insulation material and preparation method thereof
CN120795540A