Road asphalt modifier and preparation method thereof

By using asphalt modifiers prepared by rubber powder, SBS particles, rubber oil and other materials, through microwave irradiation and refining, the water resistance, viscosity and production difficulty of existing rubber asphalt materials are solved, and the resistance of asphalt pavement is improved Loading and durability extend service life and reduce production costs.

CN118909456APending Publication Date: 2024-11-08GUANGXI ZHENGLU MASCH TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193758.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing rubber asphalt materials have weak water resistance, excessive viscosity, low production, difficult storage and transportation at high temperatures, high equipment investment, high operating costs, and cannot meet the high requirements of asphalt pavement materials.

Method used

The road asphalt modifier prepared from rubber powder, SBS particles, rubber oil, activator, reinforcement and stabilizer is used to treat the modified rubber powder through microwave irradiation and in-depth refining to increase its compatibility with nano-silicon oxide. Improves the storage stability, load resistance and durability of asphalt.

Benefits of technology

It improves the storage stability of asphalt, water-soaked residual stability, high and low temperature stability and viscosity, reduces the difficulty of pavement construction, extends the service life of asphalt pavement, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a road asphalt modifier and a preparation method thereof, the asphalt modifier is prepared from 4-15% by mass of rubber powder, 0.1-0.3% by mass of an activator, 1-20% by mass of a reinforcing agent and the balance of a stabilizer, the rubber oil accounts for 4-15% by mass of the rubber powder, the activator accounts for 0.1-0.3% by mass of the rubber powder, the reinforcing agent accounts for 1-20% by mass of the rubber powder, and the stabilizer accounts for 1-20% by mass of the rubber powder. The preparation method comprises the following steps: uniformly mixing and stirring the rubber powder, the rubber oil, the activating agent, the hard asphalt powder, the plastic particles and the EBS at normal temperature to obtain a mixture A; treating the mixture A for 15-40 minutes under the closed condition of 200-270 DEG C, gradually cooling to normal temperature to obtain a mixture B, and uniformly mixing and stirring the mixture B, the SBS particles and the stabilizer to obtain the asphalt modifier for the road. The modifier can be directly added and stirred for use or is produced and used by modifying asphalt through a wet method, and the prepared asphalt modifier can improve the loading resistance, durability and high and low temperature deformation resistance of a pavement and prolong the service life of the pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of asphalt pavement materials, and in particular relates to a road asphalt modifier and a preparation method thereof. Background Art

[0002] Asphalt pavement made from waste tires is one of the most popular raw materials. At present, there are many problems with rubber asphalt or rubber asphalt mixture produced from waste tires: (1) The asphalt has weak water damage resistance and excessive viscosity; (2) The production volume is low, high-temperature storage and transportation are relatively difficult, and it is easy to agglomerate; (3) The equipment investment for rubber powder processing is large, the operating cost is high, and the production is difficult. With the rapid development of highway construction, higher requirements are put forward for asphalt pavement materials, which can no longer meet the actual use requirements. Therefore, the development of a road rubber powder and its process and the effective solution and improvement of various performance requirements of existing road rubber asphalt materials have become technical problems that need to be solved in this industry. Summary of the invention

[0003] The purpose of the present invention is to provide a road asphalt modifier and a preparation method thereof. The road asphalt modifier prepared by the present invention can improve the storage stability, water immersion residual stability, high and low temperature stability and viscosity of asphalt, reduce the difficulty of road construction, and can improve the load resistance, durability, high and low temperature resistance of the road surface and extend the service life of the asphalt road surface. In order to achieve the above purpose, the present invention adopts the following technical effects:

[0004] According to one aspect of the present invention, a road asphalt modifier is provided, which is prepared from rubber powder, SBS particles, rubber oil, an activator, a reinforcing agent and a stabilizer, wherein the rubber oil accounts for 4%-15% of the weight of the rubber powder, the activator accounts for 0.1%-0.3% of the weight of the rubber powder, and the reinforcing agent accounts for 1%-20% of the weight of the rubber powder, and the reinforcing agent is at least one of hard asphalt powder, plastic particles and EBS.

[0005] The above scheme is preferred, the rubber powder is prepared by grinding waste tires into 20-60 mesh powder and modifying it, and the ash content of the rubber powder is ≤8%. In the present invention, the steps of modifying the waste tire powder are as follows: soaking, stirring, washing and drying the waste tire particles, and then grinding them into powder; taking graphene powder and dispersing it in deionized water, and then sending it into a microwave irradiation device for irradiation at 60-80°C for 20-40 minutes, and then adding sodium sulfate and ferrous sulfate in sequence according to the quality requirements, mixing and stirring for 10-30 minutes, and then taking out the microwave irradiation device to obtain a nano-silicon oxide dispersion; the mixing and stirring speed is 80-200 rpm; in the nano-silicon oxide dispersion, the organic solvent and the ground rubber powder are sequentially added according to the quality requirements, and then high-speed shear treatment is performed for 10-20 minutes, and then kneading at 120-260°C for 30-60 minutes and cooling to obtain a modified rubber powder;

[0006] In the present invention, graphene powder is dispersed in deionized water, and then sodium sulfate, ferrous sulfate and nano-silicon oxide are added and dispersed in water to form a suspension, the nano-silicon oxide is modified under microwave irradiation, and then mixed and kneaded with rubber powder, the rubber powder reacts with the modified nano-silicon oxide dispersion, which can reduce the generation of harmful gases and enable the rubber powder to be distributed in the pores of the nano-silicon oxide. Adding an organic solvent can improve the dispersion and compatibility effect between the nano-silicon oxide and the rubber powder; wherein the mass ratio of deionized water, organic solvent, sodium sulfate, ferrous sulfate and nano-silicon oxide is 1000:(100-200):(50-150):(50-150):(0.05-0.5), the graphene powder is reduced graphene oxide powder, and the specific surface area of ​​the graphene powder is ≥300m 2 / g; the organic solvent is at least one of ethanol, ethylene glycol, propanol, isopropanol, petroleum ether, N-methylpyrrolidone, and formamide; when the rubber powder of the present invention is mixed with asphalt, the compatibility and stability of the rubber powder in the asphalt can be greatly increased, and the strength and load resistance of the asphalt can be improved.

[0007] The above scheme is further preferred, the melting point of the hard asphalt is greater than 100°C and the density is 1.02-1.5g / cm 3 .

[0008] In the above scheme, the rubber oil is at least one selected from paraffin rubber oil, aromatic rubber oil, cycloalkyl rubber oil and polycyclic aromatic rubber oil, and the activator is at least one selected from polyalkyl disulfide, alkylphenol polysulfide, phenyl disulfide and zinc salt;

[0009] The above scheme is preferred, wherein the stabilizer is a mixture of sulfur powder and a dispersant, and the mass ratio of sulfur powder to dispersant is 20:4-8, wherein the dispersant is at least one of talcum powder, calcium carbonate powder, and fly ash; the reinforcing agent is any one of hard asphalt powder, plastic particles and EBS, which can improve the high temperature performance, load resistance, etc. of asphalt, wherein EBS is vinyl bisstearamide or ethylene bisstearamide, which has multiple excellent functions such as high temperature performance and load resistance, and can also improve the viscosity, water resistance and weather resistance of asphalt; the activator shortens the regeneration time and reduces the amount of softener used in the asphalt modification production process; the cross-linking reaction of SBS particles, reinforcing agent, rubber powder and stabilizer generates macromolecules, and the sulfur-containing modified matrix improves the properties.

[0010] According to another aspect of the present invention, the present invention provides a method for preparing a road asphalt modifier, the preparation method comprising the following steps:

[0011] Weigh the following raw materials of asphalt modifier respectively by mass: rubber powder, SBS particles, rubber oil, activator, reinforcing agent and stabilizer; the reinforcing agent is at least one of hard asphalt powder, plastic particles and EBS;

[0012] The rubber powder, rubber oil, activator and reinforcing agent are mixed and stirred uniformly at room temperature to obtain a mixture A;

[0013] The mixture A is treated under a closed condition at 200-270° C. for 15-40 min, and then gradually cooled to room temperature to obtain a mixture B;

[0014] Mixing the mixture B, SBS particles and stabilizer and stirring them uniformly to obtain a road asphalt modifier;

[0015] Preferably, the rubber powder, rubber oil, activator and reinforcing agent are mixed and stirred uniformly by stirring at room temperature or under heating at 50-300 rpm;

[0016] During heating and stirring, firstly stir the rubber powder and rubber oil at 50-300 rpm, gradually heat from room temperature to 80-140°C, with the temperature rising by no more than 10°C per minute, cool to room temperature after mixing, then add the activator and reinforcing agent and mix evenly at room temperature to obtain mixture A.

[0017] Preferably, the treatment under closed conditions at 200-270° C. is performed by mixing and kneading for 15-40 minutes at a shear rate of 60-300 rpm.

[0018] Preferably, the mixture B, SBS particles and stabilizer are mixed and stirred uniformly at 50-200 rpm.

[0019] In summary, the present invention adopts the above technical solution, and the present invention has the following technical effects:

[0020] The road-used modified asphalt rubber powder of the present invention can improve the storage stability, water immersion residual stability, high and low temperature stability and viscosity of asphalt; when applied to highway construction, the road test results fully meet the national technical standards, can greatly reduce the difficulty of processing, and the road surface has the advantages of being smooth, comfortable, and low in noise; the present modifier can be used for direct mixing or produced by wet modified asphalt, and the asphalt modifier prepared by the present invention can improve the load resistance, durability, high and low temperature resistance of the road surface and extend the service life of the road surface, and greatly reduce the production cost of the asphalt modifier. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, preferred embodiments are given below to further describe the present invention in detail. However, it should be noted that many details listed in the specification are only for the purpose of enabling the reader to have a thorough understanding of one or more aspects of the present invention, and these aspects of the present invention can be implemented even without these specific details.

[0022] Example 1. This example provides a road asphalt modifier, which is prepared from rubber powder, SBS particles, rubber oil, an activator, a reinforcing agent and a stabilizer, wherein the rubber oil accounts for 4% of the rubber powder, the activator accounts for 0.1% of the rubber powder, and the reinforcing agent accounts for 20% of the rubber powder; in this example, the reinforcing agent is a hard asphalt powder, the melting point of the hard asphalt is greater than 100°C, and the density is 1.02-1.5g / cm 3 ; The rubber oil is at least one of paraffin rubber oil, aromatic rubber oil, cycloalkyl rubber oil and polycyclic aromatic rubber oil; the activator is at least one of polyalkyl disulfide, alkylphenol polysulfide, phenyl disulfide and zinc salt; the stabilizer is a mixture of sulfur powder and dispersant, the stabilizer is a mixture of sulfur powder and dispersant in a mass ratio of 4:1, and the dispersant is at least one of talcum powder, calcium carbonate powder and fly ash powder; the rubber powder is prepared by grinding waste tires into 20-60 mesh powder and modifying it, and the ash content of the rubber powder is 8%.

[0023] This embodiment provides a method for preparing a road asphalt modifier, comprising the following steps:

[0024] Step 1, weighing the following raw materials of asphalt modifier respectively by mass: rubber powder, SBS particles, rubber oil, activator, reinforcing agent and stabilizer; in this embodiment, the reinforcing agent is hard asphalt powder;

[0025] Step 2, mixing and stirring the rubber powder, rubber oil, activator and hard asphalt powder at room temperature at 300 rpm to obtain a mixture A;

[0026] Step 3, treating mixture A under a closed condition at 200° C., and gradually cooling it to room temperature to obtain mixture B; that is, mixing rubber oil with rubber powder, activator, and hard asphalt powder under a closed condition at 200° C. and a shear rate of 60 rpm for 40 minutes, and gradually cooling it to room temperature to obtain mixture B;

[0027] Step 4, mixing the mixture B, SBS particles and stabilizer at 200 rpm to obtain a road asphalt modifier;

[0028] Example 2. This example provides a road asphalt modifier, wherein the modified asphalt rubber powder is prepared from rubber powder, SBS particles, rubber oil, an activator, a reinforcing agent and a stabilizer, wherein the rubber oil accounts for 15% of the weight of the rubber powder, the activator accounts for 0.3% of the weight of the rubber powder, and the reinforcing agent accounts for 1% of the weight of the rubber powder; in this example, the reinforcing agent is selected from plastic particles, and the rubber oil is at least one of paraffin rubber oil, aromatic rubber oil, cycloalkyl rubber oil and polycyclic aromatic rubber oil; the activator is at least one of polyalkyl disulfide, alkylphenol polysulfide, phenyl disulfide and zinc salt, and the stabilizer is a mixture of sulfur powder and a dispersant in a mass ratio of 5:2; the rubber powder is prepared by grinding waste tires into 20-60 mesh powder and modifying it, and the ash content of the rubber powder is 4%.

[0029] This embodiment provides a method for preparing a road asphalt modifier, comprising the following steps:

[0030] Step 1, weighing the following raw materials of asphalt modifier respectively by mass: rubber powder, SBS particles, rubber oil, activator, reinforcing agent and stabilizer. In this embodiment, the reinforcing agent is plastic particles;

[0031] Step 2, mixing and stirring the rubber powder, rubber oil, activator and plastic particles at room temperature at 50 rpm to obtain a mixture A;

[0032] Step 3, treating the mixture A under a closed condition at 270° C., and gradually cooling it to room temperature to obtain a mixture B; that is, mixing the rubber oil with the rubber powder, the activator, and the plastic particles under a closed condition at 270° C. and a shear rate of 300 rpm for 15 minutes, and gradually cooling it to room temperature to obtain a mixture B;

[0033] Step 4, mixing the mixture B, SBS particles and stabilizer at 50 rpm to obtain a road asphalt modifier;

[0034] Example 3. This example provides a road asphalt modifier, wherein the modified asphalt rubber powder is prepared from rubber powder, SBS particles, rubber oil, an activator, a reinforcing agent and a stabilizer, wherein the rubber oil accounts for 12% of the weight of the rubber powder, the activator accounts for 0.2% of the weight of the rubber powder, and the reinforcing agent accounts for 10% of the weight of the rubber powder; the rubber oil is at least one of paraffin rubber oil, aromatic rubber oil, cycloalkyl rubber oil and polycyclic aromatic rubber oil; the activator is at least one of polyalkyl disulfide, alkylphenol polysulfide, phenyl disulfide and zinc salt, and the stabilizer is a mixture of sulfur powder and stabilizer in a mass ratio of 5:1; the rubber powder is prepared by grinding waste tires into 20-60 mesh powder and modifying it, and the ash content of the rubber powder is 5.8%.

[0035] This embodiment provides a method for preparing a road asphalt modifier, comprising the following steps:

[0036] Step 1, weighing the following raw materials of asphalt modifier respectively by mass: rubber powder, SBS particles, rubber oil, activator, reinforcing agent and stabilizer, and in this embodiment, the reinforcing agent is EBS;

[0037] Step 2, mixing and stirring the rubber powder, rubber oil, activator and EBS at 90 rpm at room temperature to obtain a mixture A;

[0038] Step 3, after treating the mixture A under a closed condition at 250° C., gradually cooling it to room temperature to obtain a mixture B; that is, after mixing and kneading the rubber oil, rubber powder, activator, and EBS under a closed condition at 250° C. and a shear rate of 120 rpm for 25 minutes, gradually cooling it to room temperature to obtain a mixture B;

[0039] Step 4: Mix the mixture B, SBS particles and stabilizer at 100 rpm and stir them evenly to obtain a road asphalt modifier.

[0040] Example 4. This example provides a road asphalt modifier, which is prepared from rubber powder, SBS particles, rubber oil, an activator, a reinforcing agent and a stabilizer, wherein the rubber oil accounts for 8% of the weight of the rubber powder, the activator accounts for 0.12% of the weight of the rubber powder, and the reinforcing agent accounts for 12% of the weight of the rubber powder; the rubber oil is at least one of paraffin rubber oil, aromatic rubber oil, cycloalkyl rubber oil and polycyclic aromatic rubber oil; the activator is at least one of polyalkyl disulfide, alkylphenol polysulfide, phenyl disulfide and zinc salt, the stabilizer is a mixture of sulfur powder and a dispersant in a mass ratio of 5:1, and the dispersant is at least one of talcum powder, calcium carbonate powder and fly ash powder; the rubber powder is prepared by grinding waste tires into 20-60 mesh powder and modifying it, and the ash content of the rubber powder is 6.1%.

[0041] This embodiment provides a method for preparing a road asphalt modifier, comprising the following steps:

[0042] Step 1, weighing the following raw materials of asphalt modifier respectively by mass: rubber powder, SBS particles, rubber oil, activator, reinforcing agent and stabilizer; in this embodiment, the reinforcing agent is hard asphalt powder;

[0043] Step 2, mixing and stirring the rubber powder, rubber oil, activator and hard asphalt powder at room temperature at 250 rpm to obtain a mixture A;

[0044] Step 3, treating mixture A under a closed condition at 240° C., and gradually cooling it to room temperature to obtain mixture B; that is, mixing rubber oil with rubber powder, activator, and hard asphalt powder under a closed condition at 240° C. and a shear rate of 250 rpm for 35 min, and gradually cooling it to room temperature to obtain mixture B;

[0045] Step 4, mixing the mixture B, SBS particles and stabilizer at 180 rpm to obtain a road asphalt modifier;

[0046] Example 5. This example provides a road asphalt modifier, which is prepared from rubber powder, SBS particles, rubber oil, an activator, a reinforcing agent and a stabilizer, wherein the rubber oil accounts for 10% of the rubber powder by weight, the activator accounts for 0.18% of the rubber powder by weight, and the reinforcing agent accounts for 18% of the rubber powder by weight. The reinforcing agent is at least one of hard asphalt powder, plastic particles and EBS; the melting point of the hard asphalt is greater than 100°C, and the density is 1.02-1.5g / cm 3The rubber oil is at least one of paraffin rubber oil, aromatic rubber oil, cycloalkyl rubber oil and polycyclic aromatic rubber oil; the activator is at least one of polyalkyl disulfide, alkylphenol polysulfide, phenyl disulfide and zinc salt; the stabilizer is a mixture of sulfur powder and dispersant in a mass ratio of 10:3, and the dispersant is at least one of talcum powder, calcium carbonate powder and fly ash powder; the rubber powder is prepared by grinding waste tires into 20-60 mesh powder and modifying it, and the ash content of the rubber powder is 6.4%.

[0047] This embodiment provides a method for preparing modified asphalt rubber powder for road use, comprising the following steps:

[0048] Step 1, weighing the following raw materials of asphalt modifier respectively by mass: rubber powder, SBS particles, rubber oil, activator, reinforcing agent and stabilizer, wherein the reinforcing agent is a mixture of two or three of hard asphalt powder, plastic particles and EBS;

[0049] Step 2, gradually heating the rubber powder and rubber oil at 80 rpm, stirring and mixing, cooling to room temperature, and then adding an activator and a reinforcing agent, and mixing at 80 rpm at room temperature to obtain a mixture A, wherein the gradually heating and stirring and mixing process is to first gradually heat the rubber powder and rubber oil at room temperature to 80-140° C. while stirring at 80 rpm, with the temperature rising by no more than 10° C. per minute, and then cooling to room temperature after the mixing is completed, and then adding the activator and the reinforcing agent and mixing at room temperature to obtain a mixture A;

[0050] Step 3, after treating the mixture A under a closed condition at 260° C., gradually cooling it to room temperature to obtain a mixture B; that is, after mixing and kneading the rubber oil, rubber powder, activator, and reinforcing agent under a closed condition at 260° C. and a shear rate of 80 rpm for 40 minutes, gradually cooling it to room temperature to obtain a mixture B;

[0051] Step 4: Mix the mixture B, SBS particles and stabilizer and stir them uniformly at 150 rpm to obtain a road asphalt modifier.

[0052] The composite modified asphalt prepared by the present invention is tested according to the "Test Procedure for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011) and JTGF40 "Technical Specifications for Highway Asphalt Pavement Construction", wherein the medium-base asphalt of the present invention uses 20# hard asphalt or 30# hard asphalt. The specific test results are shown in Table 1.

[0053] Table 1: Test results

[0054]

[0055] It can be seen from Table 1 that the road asphalt rubber powder in Examples 1-5 is higher than the technical requirements in terms of modified softening point, stability, residual stability after immersion in water, and ductility at 5°C. After the rubber powder of the present invention is applied to asphalt highway pavement construction, it can be seen that the stability, residual stability after immersion in water, and dynamic stability at 60°C and 0.7Mpa can meet the technical requirements. The segregation index of the asphalt rubber powder of the present invention can meet the technical requirements of JTGF40 "Technical Specifications for Highway Asphalt Pavement Construction", so that the storage stability of the asphalt rubber powder is effectively improved, the quality of the modified asphalt rubber powder is guaranteed, the segregation index characterizing the storage stability is improved, and the asphalt rubber powder is effectively prevented from agglomerating; it can further illustrate that the composite asphalt of the present invention can significantly improve the quality of the pavement, reduce the difficulty of pavement construction, and can improve the load resistance, durability, high and low temperature resistance of the pavement and extend the service life of the asphalt pavement.

[0056] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A road asphalt modifier, characterized in that: The road asphalt modifier is prepared from rubber powder, SBS particles, rubber oil, an activator, a reinforcing agent and a stabilizer, wherein the rubber oil accounts for 4%-15% of the rubber powder by weight, the activator accounts for 0.1%-0.3% of the rubber powder by weight, and the reinforcing agent accounts for 1%-20% of the rubber powder by weight. The reinforcing agent is a mixture of at least one or more of hard asphalt powder, plastic particles and EBS.

2. A road asphalt modifier according to claim 1, characterized in that: The rubber powder is prepared by grinding waste tires into powder with a mesh size of 20-60 and then modifying the powder. The ash content of the rubber powder is ≤8%.

3. A road asphalt modifier according to claim 1, characterized in that: The melting point of the hard asphalt is greater than 100°C and the density is 1.02-1.5 g / cm 3 .

4. A road asphalt modifier according to claim 1, characterized in that: The rubber oil is at least one of paraffin rubber oil, aromatic rubber oil, cycloalkyl rubber oil and polycyclic aromatic rubber oil, and the activator is at least one of polyalkyl disulfide, alkylphenol polysulfide, phenyl disulfide and zinc salt.

5. A road asphalt modifier according to claim 1, characterized in that: The stabilizer is a mixture of sulfur powder and a dispersant, and the dispersant is at least one of talcum powder, calcium carbonate powder and fly ash powder.

6. A method for preparing a road asphalt modifier according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: The following raw materials of asphalt modifier are weighed respectively by mass: rubber powder, SBS particles, rubber oil, activator, reinforcing agent and stabilizer; the reinforcing agent is a mixture of at least one or more of hard asphalt powder, plastic particles and EBS; The rubber powder, rubber oil, activator and reinforcing agent are mixed and stirred uniformly to obtain a mixture A; The mixture A is treated under a closed condition at 200-270° C. for 15-40 min, and then gradually cooled to room temperature to obtain a mixture B; The mixture B, SBS particles and stabilizer are mixed and stirred uniformly to obtain a road asphalt modifier.