Formula of anti-sticking coating for industrial production
By preparing a anti-adhesive coating formula containing resins, pigments, solvents and additives, the problems of insufficient adhesion, boiling resistance, aging resistance and anti-adhesive properties of traditional coatings are solved, and a variety of metal bases are realized The high adhesion and durability on the material meet the high performance needs of modern industry.
Patent Information
- Application Number
- CN202411150299.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional metal coatings have shortcomings in adhesion, boiling resistance, aging resistance, corrosion resistance and anti-stick properties, and are complex in construction and poor in adaptability, making it difficult to meet the high requirements of modern industry.
Using an anti-stick coating formula for industrial production, including resins, pigments, solvents and additives, it is prepared with high adhesion, boiling resistance and aging resistance through specific stirring, refining, filtration and vacuum defoaming processes. and paint with good anti-stick properties.
It achieves high adhesion on metal substrates such as stainless steel, aluminum alloy and cast iron. It can withstand boiling time up to 51 hours, anti-stickness up to 95%, and aging resistance up to 2250 hours, significantly improving the durability of the coating. and protective performance simplifies the construction process.
Smart Images

Figure CN118909531A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-stick coatings, in particular to a formula of anti-stick coatings for industrial production. Background Art
[0002] With the continuous development of industrial technology, various metal materials are widely used in industrial production, such as stainless steel, aluminum alloy and cast iron. These metal materials usually need to be coated with a protective coating on their surface to improve their corrosion resistance, wear resistance and aesthetics. However, traditional metal coating technology has some shortcomings in practical applications and is difficult to meet the high requirements of modern industry.
[0003] The shortcomings of existing technologies include:
[0004] Insufficient adhesion:
[0005] The adhesion of traditional metal coatings on different substrates is often not ideal, resulting in the coating being easily peeled off and falling off. This not only affects the appearance of the product, but may also cause the substrate to be directly exposed to the corrosive environment, shortening the service life of the product.
[0006] Poor boiling resistance:
[0007] Many traditional coatings are prone to hydrolysis or deterioration when exposed to water or humid environments for a long time, which reduces the protective performance of the coating. This defect is particularly obvious in industrial applications that require frequent cleaning or are in high humidity environments.
[0008] Poor aging and corrosion resistance:
[0009] Some traditional coatings are prone to aging, fading and performance degradation when exposed to ultraviolet rays, oxygen and chemical corrosive substances for a long time, affecting the long-term protection effect of the coating. In addition, insufficient anti-corrosion performance is also a major shortcoming of traditional coatings, which cannot provide adequate protection in harsh chemical environments.
[0010] Poor anti-stick performance:
[0011] The anti-stick performance of traditional coatings is often not ideal, and they are prone to adhere to dust, oil and other impurities, which increases the difficulty of cleaning and maintenance and affects the normal operation and service life of the equipment.
[0012] Complex construction and poor adaptability:
[0013] The preparation and construction processes of many traditional coatings are complex and difficult to apply directly on existing production lines, requiring additional equipment and process adjustments. In addition, the formula adaptability of traditional coatings is poor, and it is difficult to flexibly adjust according to different substrates and usage environments, which limits its scope of application. Summary of the invention
[0014] In view of the deficiencies of the prior art, the present invention provides a formula for an anti-stick coating for industrial production, which solves the problems of the prior art such as insufficient adhesion, poor boiling resistance, poor aging resistance and corrosion resistance, poor anti-stick performance, complex construction and poor adaptability.
[0015] To achieve the above purpose, the present invention is implemented through the following technical scheme: a formula of an anti-stick coating for industrial production, which includes 55-59.5 parts of resin, 7-15 parts of pigment, 2.3-2.86 parts of solvent, and 3-3.85 parts of additives by weight.
[0016] Preferably, the resin includes 25-30 parts of polyurethane resin, 10-20 parts of thermosetting acrylic resin, 3-5 parts of fully etherified amino resin, 3-8 parts of fluorocarbon resin, and 5-10 parts of silicone resin.
[0017] Preferably, the solvent includes 0.44-0.56 parts of cyclohexanone, 0.45-0.5 parts of xylene, 0.8-1.0 parts of butyl ester, and 0.98-1.0 parts of methyl isobutyl ketone.
[0018] Preferably, the auxiliary agent includes 0.8-1.0 parts of leveling agent, 1.7-2.0 parts of defoaming agent, and 0.7-1.5 parts of dispersant.
[0019] Preferably, the pigment is an electron transfer type organic compound.
[0020] Preferably, the leveling agent is a fluorine-modified leveling agent, the defoaming agent is a silicon-based defoaming agent, and the dispersant is a high-molecular copolymer alkyl ammonium salt dispersant.
[0021] A method for preparing an anti-sticking coating for industrial production, using an anti-sticking coating formula for industrial production, comprises the following steps:
[0022] S1. Resin pretreatment: polyurethane resin, thermosetting acrylic resin, fully etherified amino resin, fluorocarbon resin and silicone resin are stirred evenly at room temperature, and appropriate amounts of cyclohexanone, xylene, butyl ester and methyl isobutyl ketone are added during the stirring process to reduce the viscosity of the resin;
[0023] S2, main mixing process: add the pretreated resin component into the mixing tank, start stirring at a low speed and slowly add the pigment, gradually add the remaining solvent after the pigment is dispersed and fused with the resin, and finally add the leveling agent, defoamer and dispersant into the mixing tank in sequence, continue stirring until the mixture is uniform, and obtain a mixed solution A;
[0024] S3, refinement: the mixed solution A is refined by a refiner to obtain a mixed solution B;
[0025] S4, filtration: Use a filter with a mesh size of 300 or more to filter the mixed solution B to remove particles and impurities in the mixing process, ensure the uniformity and purity of the mixed solution B, and obtain a mixed solution C;
[0026] S5, vacuum degassing: the filtered mixed liquid C is transferred to a vacuum degassing machine, and degassing is performed under low temperature conditions to ensure that there are no bubbles in the mixed liquid C, thereby obtaining a coating;
[0027] S6. Packaging and storage: As required, the prepared coating is sealed and packaged and stored in a cool and dry environment.
[0028] Preferably, in the S2 step, the speed of the initial stage of low-speed stirring is 100-150RPM, the stirring time is 10-15min, the speed of the pigment adding stage is 150-200RPM, the stirring time is 15-30min, and the speed of the remaining solvent adding stage is 150-200RPM, and the stirring time is 5-10min.
[0029] Preferably, the refinement size in step S3 reaches 20-30 μm.
[0030] Preferably, in the step S5, the vacuum degree of the vacuum degassing machine is set to 50-100 kPa, the temperature is set to 20° C.-30° C., the stirring speed is 50-100 RPM, and the degassing time is 30-60 min.
[0031] The present invention provides a formula of anti-stick coating for industrial production. It has the following beneficial effects:
[0032] 1. The adhesion test results of the anti-stick coating of the present invention on metal substrates such as stainless steel, aluminum alloy, and cast iron show that the coating can achieve high adhesion on different metal substrates, ensuring the firm adhesion of the coating film on various substrates, and is suitable for a variety of industrial applications.
[0033] 2. The coating of the present invention performs well in the water boiling resistance test, with a water boiling resistance time of up to 51 hours. It is suitable for environments that require long-term contact with water to ensure the durability of the coating. The anti-stick test shows that the coating of the present invention has good anti-stick properties, with an anti-stick property of up to 95%, which significantly reduces the possibility of surface contamination, facilitates cleaning and maintenance, and improves the use efficiency and life of industrial equipment.
[0034] 3. The anti-stick coating of the present invention performs well in the interlayer adhesion test and has strong interlayer adhesion, so that the coating can be recoated multiple times without affecting the overall performance, and is particularly suitable for industrial products that require multiple coatings.
[0035] 4. The coating of the present invention performs excellently in aging resistance and corrosion resistance tests, with an aging resistance time of up to 2250 hours and a corrosion resistance time of up to 1800 hours, ensuring the long-term stability and protective performance of the coating in harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the process steps of the present invention. DETAILED DESCRIPTION
[0037] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Please see attached Figure 1 The embodiment of the present invention provides a formula of an anti-stick coating for industrial production, which includes 55-59.5 parts of resin, 7-15 parts of pigment, 2.3-2.86 parts of solvent, and 3-3.85 parts of auxiliary agent by weight. The pigment is an electron transfer type organic compound.
[0039] The leveling agent adopts fluorine-modified leveling agent, the defoaming agent adopts silicon defoaming agent, and the dispersant adopts high molecular copolymer alkyl ammonium salt dispersant.
[0040] The resin comprises 25-30 parts of polyurethane resin, 10-20 parts of thermosetting acrylic resin, 3-5 parts of fully etherified amino resin, 3-8 parts of fluorocarbon resin and 5-10 parts of silicone resin.
[0041] The solvent includes 0.44-0.56 parts of cyclohexanone, 0.45-0.5 parts of xylene, 0.8-1.0 parts of butyl ester, and 0.98-1.0 parts of methyl isobutyl ketone.
[0042] The additives include 0.8-1.0 parts of leveling agent, 1.7-2.0 parts of defoaming agent and 0.7-1.5 parts of dispersant.
[0043] A method for preparing an anti-sticking coating for industrial production comprises the following steps:
[0044] S1. Resin pretreatment: polyurethane resin, thermosetting acrylic resin, fully etherified amino resin, fluorocarbon resin and silicone resin are stirred evenly at room temperature, and appropriate amounts of cyclohexanone, xylene, butyl ester and methyl isobutyl ketone are added during the stirring process to reduce the viscosity of the resin;
[0045] S2, main mixing process: add the pretreated resin component into the mixing tank, start stirring at a low speed and slowly add the pigment, gradually add the remaining solvent after the pigment is dispersed and fused with the resin, and finally add the leveling agent, defoamer and dispersant into the mixing tank in sequence, continue stirring until the mixture is uniform, and obtain a mixed solution A;
[0046] In step S2, the initial stage of low-speed stirring has a rotation speed of 100-150RPM, the stirring time is 10-15min, the pigment adding stage has a rotation speed of 150-200RPM, the stirring time is 15-30min, and the remaining solvent adding stage has a rotation speed of 150-200RPM, the stirring time is 5-10min.
[0047] S3, refinement: The mixed solution A is refined by a refiner to obtain a mixed solution B; the refinement size in step S3 reaches 20-30 μm.
[0048] S4, filtration: Use a filter with a mesh size of 300 or more to filter the mixed solution B to remove particles and impurities in the mixing process, ensure the uniformity and purity of the mixed solution B, and obtain a mixed solution C;
[0049] S5, vacuum degassing: transfer the filtered mixed liquid C to a vacuum degassing machine, and perform degassing treatment under low temperature conditions to ensure that there are no bubbles in the mixed liquid C to obtain the coating; in step S5, the vacuum degree of the vacuum degassing machine is set to 50-100 kPa, the temperature is set to 20°C-30°C, the stirring speed is 50-100 RPM, and the degassing time is 30-60 min.
[0050] S6. Packaging and storage: As required, the prepared coating is sealed and packaged and stored in a cool and dry environment.
[0051] Example 1
[0052] formula:
[0053] Resin: 55 parts
[0054] Polyurethane resin: 25 parts
[0055] Thermosetting acrylic resin: 10 parts
[0056] Fully etherified amino resin: 3 parts
[0057] Fluorocarbon resin: 8 parts
[0058] Silicone resin: 9 parts
[0059] Pigment: 7 parts
[0060] Solvent: 2.3 parts
[0061] Cyclohexanone: 0.44 parts
[0062] Xylene: 0.45 parts
[0063] Butyl ester: 0.8 parts
[0064] Methyl isobutyl ketone: 0.98 parts
[0065] Additives: 3 parts
[0066] Leveling agent: 0.8 parts
[0067] Defoamer: 1.7 parts
[0068] Dispersant: 0.7 parts
[0069] Preparation steps:
[0070] S1. Resin pretreatment: polyurethane resin, thermosetting acrylic resin, fully etherified amino resin, fluorocarbon resin and silicone resin are stirred evenly at room temperature, and each resin is stirred for 5 minutes.
[0071] During the stirring process, appropriate amounts of cyclohexanone and xylene were added respectively to reduce the viscosity of the resin.
[0072] S2, main mixing process: add the pre-treated resin components into the mixing tank, stir at low speed (100-150RPM) for 10-15 minutes. Slowly add the pigment, increase the speed to 150-200RPM, stir for 15-30 minutes to ensure that the pigment is evenly dispersed. Gradually add the remaining solvent, maintain the speed of 150-200RPM, and stir for 5-10 minutes. Add the leveling agent, defoamer and dispersant in turn, continue to stir until the mixture is evenly mixed, and obtain the mixed solution A.
[0073] S3. Refining: The mixed solution A is refined by a refiner, and the refinement size reaches 20-30 μm to obtain a mixed solution B.
[0074] S4. Filtration: Use a filter with a mesh size of 300 or above to filter the mixed solution B to remove particles and impurities, ensure the uniformity and purity of the mixed solution B, and obtain a mixed solution C.
[0075] S5. Vacuum degassing: transfer the mixed liquid C to a vacuum degassing machine, set the vacuum degree to 50-100 kPa, the temperature to 20°C-30°C, the stirring speed to 50-100 RPM, and the degassing time to 30-60 minutes, ensuring that there are no bubbles in the mixed liquid C to obtain the coating.
[0076] S6. Packaging and storage: As required, the prepared coating shall be sealed and packaged and stored in a cool and dry environment.
[0077] Summary: The coating has bright color, good adhesion and excellent water boiling resistance.
[0078] Example 2
[0079] formula:
[0080] Resin: 59.5 parts
[0081] Polyurethane resin: 30 parts
[0082] Thermosetting acrylic resin: 20 parts
[0083] Fully etherified amino resin: 5 parts
[0084] Fluorocarbon resin: 3 parts
[0085] Silicone resin: 1.5 parts
[0086] Pigment: 15 parts
[0087] Solvent: 2.86 parts
[0088] Cyclohexanone: 0.56 parts
[0089] Xylene: 0.5 parts
[0090] Butyl ester: 1.0 part
[0091] Methyl isobutyl ketone: 1.0 part
[0092] Additives: 3.85 parts
[0093] Leveling agent: 1.0 part
[0094] Defoamer: 2.0 parts
[0095] Dispersant: 1.5 parts
[0096] Preparation steps:
[0097] S1. Resin pretreatment: Stir the resin components evenly at room temperature for 10 minutes for each resin. During the stirring process, add appropriate amounts of cyclohexanone and xylene.
[0098] S2, main mixing process: add the pretreated resin component to the mixing tank, stir at low speed (100-150RPM) for 15 minutes. Slowly add the pigment, increase the speed to 150-200RPM, and stir for 20 minutes. Gradually add the remaining solvent, keep the speed at 150-200RPM, and stir for 10 minutes. Add the leveling agent, defoamer and dispersant in sequence, continue to stir until the mixture is uniform, and obtain the mixed solution A.
[0099] S3. Refining: The mixed solution A is refined by a refiner, and the refinement size reaches 20-30 μm to obtain a mixed solution B.
[0100] S4. Filtration: Filter the mixed solution B using a filter screen with a mesh size of 300 or more to ensure uniformity and purity, thereby obtaining a mixed solution C.
[0101] S5. Vacuum degassing: the vacuum degree is set to 50-100 kPa, the temperature is set to 20°C-30°C, the stirring speed is 50-100 RPM, and the degassing time is 40 minutes.
[0102] S6. Packaging and storage: As required, the prepared coating shall be sealed and packaged and stored in a cool and dry environment.
[0103] Summary: Coating adhesion and corrosion resistance are significantly improved.
[0104] Example 3
[0105] formula:
[0106] Resin: 57 parts
[0107] Polyurethane resin: 28 parts
[0108] Thermosetting acrylic resin: 15 parts
[0109] Fully etherified amino resin: 4 parts
[0110] Fluorocarbon resin: 5 parts
[0111] Silicone resin: 5 parts
[0112] Pigment: 12 parts
[0113] Solvent: 2.5 parts
[0114] Cyclohexanone: 0.5 parts
[0115] Xylene: 0.47 parts
[0116] Butyl ester: 0.83 parts
[0117] Methyl isobutyl ketone: 1.0 part
[0118] Additives: 3.5 parts
[0119] Leveling agent: 0.9 parts
[0120] Defoamer: 1.8 parts
[0121] Dispersant: 0.8 parts
[0122] Preparation steps:
[0123] S1. Resin pretreatment: Stir the resin components evenly at room temperature for 8 minutes for each resin. During the stirring process, add appropriate amounts of cyclohexanone and xylene.
[0124] S2, main mixing process: add the pretreated resin component to the mixing tank, stir at low speed (120RPM) for 10 minutes. Slowly add the pigment, increase the speed to 180RPM, and stir for 25 minutes. Gradually add the remaining solvent, maintain the speed at 180RPM, and stir for 8 minutes. Add the leveling agent, defoamer and dispersant in sequence, continue to stir evenly, and obtain mixed solution A.
[0125] S3. Refining: The mixed solution A is refined by a refiner, and the refinement size reaches 25 μm to obtain a mixed solution B.
[0126] S4. Filtration: Filter the mixed solution B using a filter screen with a mesh size of 350 or above to ensure uniformity and purity, thereby obtaining a mixed solution C.
[0127] S5. Vacuum degassing: the vacuum degree is set to 60-80 kPa, the temperature is set to 25°C, the stirring speed is 70 RPM, and the degassing time is 50 minutes.
[0128] S6. Packaging and storage: As required, the prepared coating shall be sealed and packaged and stored in a cool and dry environment.
[0129] Summary: The interlayer adhesion and aging resistance of the coating are enhanced.
[0130] Example 4
[0131] formula:
[0132] Resin: 56 parts
[0133] Polyurethane resin: 26 parts
[0134] Thermosetting acrylic resin: 12 parts
[0135] Fully etherified amino resin: 4 parts
[0136] Fluorocarbon resin: 7 parts
[0137] Silicone resin: 7 parts
[0138] Pigment: 10 parts
[0139] Solvent: 2.7 parts
[0140] Cyclohexanone: 0.54 parts
[0141] Xylene: 0.48 parts
[0142] Butyl ester: 0.85 parts
[0143] Methyl isobutyl ketone: 1.03 parts
[0144] Additives: 3.3 parts
[0145] Leveling agent: 0.85 parts
[0146] Defoamer: 1.75 parts
[0147] Dispersant: 0.7 parts
[0148] Preparation steps:
[0149] S1. Resin pretreatment: Stir polyurethane resin, thermosetting acrylic resin, fully etherified amino resin, fluorocarbon resin and silicone resin at room temperature for 8 minutes respectively. Add cyclohexanone and xylene and continue stirring for 10 minutes to reduce the viscosity.
[0150] S2, main mixing process: add the pretreated resin component to the mixing tank, stir at a low speed of 100RPM in the initial stage, and stir for 12 minutes. Slowly add the pigment, increase the speed to 150RPM, and stir for 20 minutes. Gradually add the remaining solvent, keep the speed at 150RPM, and stir for 10 minutes. Finally, add the leveling agent, defoamer and dispersant in turn, and continue stirring for 20 minutes to obtain a mixed solution A.
[0151] S3. Refining: The mixed solution A is processed by a refiner to a size of 20 μm to obtain a mixed solution B.
[0152] S4, filtration: Filter the mixed solution B using a filter screen with a mesh size of 300 or more to obtain a mixed solution C.
[0153] S5. Vacuum degassing: transfer the mixed liquid C to a vacuum degassing machine, set the vacuum degree to 50 kPa, the temperature to 25°C, the stirring speed to 60 RPM, and the degassing time to 40 minutes to ensure that there are no bubbles to obtain the coating.
[0154] S6. Packaging and storage: The prepared coating should be sealed and stored in a cool and dry environment.
[0155] Summary: The chemical resistance and mechanical properties of the coating are improved.
[0156] Example 5
[0157] formula:
[0158] Resin: 58 parts
[0159] Polyurethane resin: 29 parts
[0160] Thermosetting acrylic resin: 18 parts
[0161] Fully etherified amino resin: 4 parts
[0162] Fluorocarbon resin: 4 parts
[0163] Silicone resin: 3 parts
[0164] Pigment: 13 parts
[0165] Solvent: 2.6 parts
[0166] Cyclohexanone: 0.55 parts
[0167] Xylene: 0.47 parts
[0168] Butyl ester: 0.85 parts
[0169] Methyl isobutyl ketone: 0.98 parts
[0170] Additives: 3.75 parts
[0171] Leveling agent: 0.95 parts
[0172] Defoamer: 1.85 parts
[0173] Dispersant: 0.95 parts
[0174] Preparation steps:
[0175] S1. Resin pretreatment: Stir polyurethane resin, thermosetting acrylic resin, fully etherified amino resin, fluorocarbon resin and silicone resin at room temperature for 10 minutes respectively. Add cyclohexanone and xylene and continue stirring for 15 minutes to reduce the viscosity.
[0176] S2, main mixing process: add the pretreated resin component to the mixing tank, stir at a low speed of 150RPM in the initial stage, and stir for 15 minutes. Slowly add the pigment, increase the speed to 200RPM, and stir for 25 minutes. Gradually add the remaining solvent, keep the speed at 200RPM, and stir for 10 minutes. Finally, add the leveling agent, defoamer and dispersant in turn, and continue stirring for 15 minutes to obtain a mixed solution A.
[0177] S3. Refining: The mixed solution A is processed by a refiner to a size of 25 μm to obtain a mixed solution B.
[0178] S4, filtration: Filter the mixed solution B using a filter screen with a mesh size of 400 or more to obtain a mixed solution C.
[0179] S5. Vacuum degassing: transfer the mixed liquid C to a vacuum degassing machine, set the vacuum degree to 70 kPa, the temperature to 20°C, the stirring speed to 70 RPM, and the degassing time to 45 minutes, ensuring that there are no bubbles, to obtain the coating.
[0180] S6. Packaging and storage: The prepared coating should be sealed and stored in a cool and dry environment.
[0181] Summary: The coating has excellent temperature resistance and weather resistance.
[0182] Summary
[0183] Example 1: Overall balance, suitable for a variety of occasions.
[0184] Example 2: Optimal adhesion and corrosion resistance.
[0185] Example 3: The interlayer adhesion and aging resistance are strong.
[0186] Example 4: Outstanding chemical resistance and mechanical properties.
[0187] Example 5: Excellent heat resistance and weather resistance.
[0188] Comparative Experimental Design and Data
[0189] Comparative experiment 1: Effect of different resin ratios
[0190]
[0191] Comparative experiment 2: Effect of different pigment contents
[0192]
[0193] Comparative experiment 3: Effect of different solvent ratios
[0194]
[0195] Experimental Summary
[0196] Through the above table and the data of the comparative experiments, we can clearly see the unique advantages and room for improvement of each embodiment.
[0197] To summarize:
[0198] Embodiment 1: The overall performance is balanced and suitable for a variety of occasions.
[0199] Example 2: performs best in terms of adhesion and corrosion resistance.
[0200] Example 3: Excellent interlayer adhesion and aging resistance.
[0201] Example 4: Outstanding chemical resistance and mechanical properties.
[0202] Example 5: has significant advantages in temperature resistance and weather resistance.
[0203] Anti-stick test method:
[0204] The anti-adhesion test uses a standard experimental method to attach a specific adhesive material to the surface of the coating film and then measure the adhesion using a tensile tester to calculate the anti-adhesion percentage.
[0205] Summary of comparative experimental results
[0206] In the experiments with different resin, pigment and solvent ratios, we saw different anti-stick performances, as follows:
[0207] Influence of resin ratio: Sample A with high polyurethane content has lower anti-stick properties, while sample B with high thermosetting acrylic resin content has higher anti-stick properties.
[0208] Effect of Pigment Content: Comparative Sample D with high pigment content exhibits the best anti-stick properties.
[0209] Effect of solvent ratio: Comparative sample F with optimized solvent ratio showed the best anti-sticking performance.
[0210] Through these experiments and comparisons, we can clearly conclude the best choice for each formulation in different application scenarios.
[0211] Test results for different metal substrates
[0212] In order to fully demonstrate the performance of the anti-stick coating of the present invention on different metal substrates, we selected three common industrial substrates for testing: stainless steel, aluminum alloy and cast iron.
[0213] Test items
[0214] 1. Adhesion test
[0215] 2. Boiling resistance test
[0216] 3. Aging resistance test
[0217] 4. Corrosion resistance test
[0218] 5. Anti-stickiness test
[0219] Stainless steel substrate
[0220]
[0221] Aluminum alloy substrate
[0222]
[0223] Cast iron substrate
[0224]
[0225] Summary
[0226] Through the tests on different metal substrates, we can see the excellent performance of the anti-stick coating of the present invention on different substrates:
[0227] Stainless steel substrate: Excellent performance, especially Example 5, with the highest adhesion and corrosion resistance, excellent anti-stick performance, suitable for high-demand stainless steel surface protection.
[0228] Aluminum alloy substrate: performed well. Examples 2 and 5 performed outstandingly in adhesion and corrosion resistance, and are suitable for the protection and decoration of aluminum alloy products.
[0229] Cast iron substrate: The performance is also excellent. Example 5 has the best performance in terms of adhesion, corrosion resistance and anti-sticking properties, and is suitable for the protection of cast iron products.
[0230] Main conclusions
[0231] Adhesion: All examples achieved high levels of adhesion on different metal substrates, ensuring the firmness and stability of the coating.
[0232] Water boiling resistance: On different metal substrates, the water boiling resistance is good, suitable for long-term exposure to water or humid environment.
[0233] Aging resistance: Test results show that the coating has excellent aging resistance on various substrates and is suitable for long-term use.
[0234] Corrosion resistance: The coating exhibits excellent corrosion resistance on all substrates, especially stainless steel and cast iron substrates, ensuring protection in harsh environments.
[0235] Anti-stick properties: Anti-stick test results show that the coating can significantly reduce contamination and adhesion on different metal substrates, making it easier to clean and maintain.
[0236] Through these test data and comparative analysis, we can clearly see that the anti-stick coating of the present invention has excellent performance on a variety of metal substrates, meeting the needs of modern industry for high-performance anti-stick coatings.
[0237] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A formulation of an anti-stick coating for industrial production, characterized in that: By weight, the composition comprises 55-59.5 parts of resin, 7-15 parts of pigment, 2.3-2.86 parts of solvent and 3-3.85 parts of auxiliary agent.
2. The anti-stick coating formulation for industrial production according to claim 1, characterized in that: The resin comprises 25-30 parts of polyurethane resin, 10-20 parts of thermosetting acrylic resin, 3-5 parts of fully etherified amino resin, 3-8 parts of fluorocarbon resin and 5-10 parts of silicone resin.
3. The anti-stick coating formulation for industrial production according to claim 1, characterized in that: The solvent comprises 0.44-0.56 parts of cyclohexanone, 0.45-0.5 parts of xylene, 0.8-1.0 parts of butyl ester and 0.98-1.0 parts of methyl isobutyl ketone.
4. The anti-stick coating formulation for industrial production according to claim 1, characterized in that: The auxiliary agent includes 0.8-1.0 parts of leveling agent, 1.7-2.0 parts of defoaming agent and 0.7-1.5 parts of dispersant.
5. The anti-stick coating formulation for industrial production according to claim 1, characterized in that: The pigment is an electron transfer type organic compound.
6. The anti-stick coating formulation for industrial production according to claim 4, characterized in that: The leveling agent is a fluorine-modified leveling agent, the defoaming agent is a silicon-based defoaming agent, and the dispersant is a high-molecular copolymer alkyl ammonium salt dispersant.
7. A method for preparing an anti-sticking coating for industrial production, characterized in that: The industrial production anti-sticking coating formulation according to any one of claims 1 to 6 comprises the following steps: S1. Resin pretreatment: polyurethane resin, thermosetting acrylic resin, fully etherified amino resin, fluorocarbon resin and silicone resin are stirred evenly at room temperature, and appropriate amounts of cyclohexanone, xylene, butyl ester and methyl isobutyl ketone are added during the stirring process to reduce the viscosity of the resin; S2, main mixing process: add the pretreated resin component into the mixing tank, start stirring at a low speed and slowly add the pigment, gradually add the remaining solvent after the pigment is dispersed and fused with the resin, and finally add the leveling agent, defoamer and dispersant into the mixing tank in sequence, continue stirring until the mixture is uniform, and obtain a mixed solution A; S3, refinement: the mixed solution A is refined by a refiner to obtain a mixed solution B; S4, filtration: Use a filter with a mesh size of 300 or more to filter the mixed solution B to remove particles and impurities in the mixing process, ensure the uniformity and purity of the mixed solution B, and obtain a mixed solution C; S5, vacuum degassing: the filtered mixed liquid C is transferred to a vacuum degassing machine, and degassing is performed under low temperature conditions to ensure that there are no bubbles in the mixed liquid C, thereby obtaining a coating; S6. Packaging and storage: As required, the prepared coating is sealed and packaged and stored in a cool and dry environment.
8. The method for preparing an anti-sticking coating for industrial production according to claim 7, characterized in that: In the step S2, the initial stage of low-speed stirring has a rotation speed of 100-150RPM, the stirring time is 10-15min, the pigment adding stage has a rotation speed of 150-200RPM, the stirring time is 15-30min, and the remaining solvent adding stage has a rotation speed of 150-200RPM, the stirring time is 5-10min.
9. The method for preparing an anti-sticking coating for industrial production according to claim 7, characterized in that: In the S3 step, the refined size reaches 20-30 μm.
10. The method for preparing an anti-sticking coating for industrial production according to claim 7, characterized in that: In the step S5, the vacuum degree of the vacuum degassing machine is set to 50-100 kPa, the temperature is set to 20° C.-30° C., the stirring speed is 50-100 RPM, and the degassing time is 30-60 min.