High-toughness epoxy polysilsesquioxane optical coating and preparation method thereof
High-tough epoxy polysilsesquioxane optical by introducing long-chain flexible molecules between polysilsesquioxane monomer molecules, combining epoxy polysilsesquioxane, softening and toughening agent and photoinitiator, prepare high-toughening epoxy polysilsesquioxane optical The coating solves the problem of insufficient flexibility of polysilsesquioxane coating and achieves high hardness and high wear resistance on the folding screen cover.
Patent Information
- Application Number
- CN202410988508.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The existing polysilsesquioxane coatings are prone to cracks in small bending radius or external bending, and have poor flexibility, which cannot meet the high hardness and wear resistance requirements of the folding screen cover.
High tough epoxy polysesquioxane monomer molecules are prepared by introducing long-chain flexible molecules between polysilsesquioxane monomer molecules, combining epoxy polysilsesquioxane, softening and toughening agent, photoinitiator and solvent. The optical coating of oxane adopts roller coating and UV curing processes to form a coating with both hardness and toughness.
While maintaining high strength and high thermal stability, the toughness of the coating is significantly improved, suitable for folding screen cover protection materials, enhancing its performance under small bending and external bending conditions.
Smart Images

Figure BDA0004958200470000041 
Figure BDA0004958200470000042 
Figure BDA0004958200470000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polysilsesquioxane optical coatings, and in particular to a high-toughness epoxy polysilsesquioxane optical coating and a preparation method thereof. Background Art
[0002] Foldable devices have attracted widespread attention from users because of their advantages of large screens and portability. The cover is not only the interface for human-computer interaction, but also a protective barrier for flexible OLEDs, which deeply affects the user experience. It is also one of the bottleneck materials that restrict the development of folding device technology. At present, there are three main screen cover materials for folding screens: UTG (Ultra-Thin-Glass), CPI (transparent polyimide), and PET (polyethylene terephthalate). UTG has both ultra-high hardness and bending resistance, and its touch and scratch resistance are closer to the glass cover of traditional mobile phones, but due to its fragile nature, it cannot be applied to the first surface of human-computer contact. CPI / PET, a plastic cover, has good flexibility, but its hardness is low and cannot be used directly. It is necessary to apply a layer of hardened coating on the surface to give it scratch resistance and anti-fingerprint effects. However, even the hardened coating with the best performance cannot achieve the hardness and touch of glass.
[0003] Flexible hard coatings require both hardness and toughness. Based on current application results, they can be roughly divided into three categories: organic, inorganic, and organic-inorganic hybrid coatings. Among them, organic-inorganic hybrid coatings have become a current research hotspot because they can achieve both glass-like wear resistance and plastic-like flexibility, and are expected to be used as flexible touch screen cover coatings; while polysilsesquioxane coatings have high hardness and high wear resistance while still maintaining their flexibility and high transparency, making them a material with great potential.
[0004] Invention patent CN114702900B discloses a coating liquid compounded by organic siloxane and modified POSS. The coating is used on the surface of the glass back cover of mobile phones, which can obtain moderate smoothness, excellent moderate hydrophobic cleaning ability and wear resistance. Invention patent CN111454648B discloses a coating with naphthalene ring type polyethylene glycol acrylate as the main body and octavinyl-POSS compounded. The number of bending times of the coating is not limited, the bending resistance is good, and the wear resistance is good. Invention patent CN114539915A discloses a polysilsesquioxane with epoxy functional groups as the main body, which has low shrinkage, high hardness, flexibility, and anti-fingerprint hardening coating.
[0005] The above technologies all use polysilsesquioxane, among which the coating with polysilsesquioxane as the main body has high hardness, but insufficient toughness; while using polysilsesquioxane as a modification aid maintains its toughness, but cannot exert its hardness advantage. In addition to the shortcomings of the existing technology, on the other hand, as the bending angle requirements become smaller and smaller, conventional polysilsesquioxane is difficult to meet the demand, especially for external bending. Therefore, how to improve its toughness while maintaining the original hardness, wear resistance and transparency is a problem that needs to be solved urgently. . Summary of the invention
[0006] The purpose of the present invention is to solve the problems of poor flexibility of polysilsesquioxane coatings in the prior art, and the easy generation of cracks in small bending radius or external bending. Provide a high-toughness epoxy polysilsesquioxane optical coating, by introducing long-chain flexible molecules between polysilsesquioxane monomer molecules, while maintaining the original high strength, hardness, high thermal stability and many other excellent properties, improve its material toughness, and realize its application in folding screen cover protective materials.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] A high-toughness epoxy polysilsesquioxane optical coating, the raw materials of which include epoxy polysilsesquioxane, a flexibility and toughening agent, a photoinitiator and a solvent.
[0009] Specifically, the total weight proportion of each raw material is: epoxy polysilsesquioxane 40-85wt%, solvent 10-50wt%, flexibility and toughening agent 0.5-15wt%, photoinitiator 0.5-2wt%.
[0010] Furthermore, the epoxy-containing polysilsesquioxane is a cage-shaped polysilsesquioxane POSS or a ladder-shaped polysilsesquioxane LPSQ or a random polysilsesquioxane; the epoxy functional group includes epoxy cyclohexyl and glycidyl ether oxypropyl, and the epoxy functional group is a bifunctional group or a multifunctional group.
[0011] Specifically, the photoinitiator is at least one of an onium salt initiator, a metal organic initiator, and an organosilane initiator, preferably an onium salt initiator; the solvent is at least one of 2-butanone, ethyl acetate, and propylene glycol methyl ether acetate.
[0012] Specifically, the flexibility and toughening agent is one or more of mono / bi-terminal epoxy polyether silicone oil (Mw≤2k), mono / bi-terminal epoxy polyether (Mw≤3k), mono / bi-terminal hydroxyl polyether silicone oil (Mw≤2k), mono / bi-terminal hydroxyl-terminated polyether (Mw≤3k), ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0013] The present invention also provides a method for preparing the above-mentioned high-toughness epoxy polysilsesquioxane optical coating, comprising the following steps:
[0014] Step 1, adding epoxy polysilsesquioxane, a flexibilizer and a photoinitiator to a solvent in sequence, stirring continuously until uniform, to obtain a formula slurry;
[0015] Step 2: coating the obtained formula slurry on the surface of the substrate, and then drying the solvent and UV curing, so as to form an optical coating with both hardness and toughness on the surface of the substrate.
[0016] Specifically, the stirring speed in step 1 is 200-300 rpm, the epoxy polysilsesquioxane is added to the solvent and stirred for 30-60 minutes, then the flexibility and toughness enhancer is added and stirred for 40-50 minutes, and finally the photoinitiator is added and stirred for 30-60 minutes until the solution is uniformly stirred to obtain a formula slurry.
[0017] Preferably, the coating method in step 2 is any one of roller coating, blade coating, dip coating, wheel coating, spin coating, and slit coating.
[0018] Specifically, the drying temperature in step 2 is 60-110°C, the drying time is 20-90 min, and the radiation dose of the UV curing is 700-2000 mJ / cm 2 .
[0019] Preferably, the substrate in step 2 is at least one of a CPI substrate, a PET substrate, and polymethyl methacrylate (PMMA).
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention introduces long-chain flexible molecules between polysilsesquioxane monomer molecules, thereby improving the toughness of the material while maintaining the original high strength, hardness, high thermal stability and many other excellent properties, thereby realizing its application in folding screen cover protective materials. DETAILED DESCRIPTION
[0022] In order to better reflect the advantages and innovations of the present invention and clearly demonstrate the technical solution of the present invention, the present invention will be further described in detail below in conjunction with specific embodiments.
[0023] Example 1
[0024] The invention provides a high-toughness epoxy polysilsesquioxane optical coating, the raw materials of which include epoxy polysilsesquioxane, a flexibilizer and a toughener, a photoinitiator and a solvent.
[0025] In this embodiment, the composition ratio of each raw material of the formula slurry is as follows (by mass percentage):
[0026]
[0027] The specific preparation method is:
[0028] Step 11, add 70g of epoxy cyclohexylethyl-cage polysilsesquioxane to 25.5g of butanone, stir at 200rpm, stir for 60min; add 3.5g of double-terminal epoxy polyether silicone oil (brand Silok8358, Mw=1k) at 300rpm, stir for 40min; add 1g of triphenyl hexafluoroantimonate, stir at 300rpm, stir for 40min, and obtain HC slurry.
[0029] Step 12: The HC slurry was coated on a 50 μm thick CPI film (purchased from Kolon, South Korea) using a scraper (speed 30 cm / min). The coated CPI film was placed in an oven at 80°C and dried for 25 min. Then, the film was heated at 1500 mJ / cm 2 After photocuring with a UV lamp with a radiation dose of 1.5 %, a HC-CPI film with a HC (hardened coating) thickness of 35 μm was obtained.
[0030] Example 2
[0031] In this embodiment, the composition ratio of each raw material of the formula slurry is as follows (by mass percentage):
[0032]
[0033] The specific preparation method is:
[0034] Step 21, add 70g of epoxycyclohexylethyl-cage polysilsesquioxane to 25.5g of butanone, stirring at a speed of 200rpm, stirring for 60min; add 3.5g of polypropylene glycol diglycidyl ether (grade 227, Mw=1k) at a stirring speed of 300rpm, stirring for 40min; add 1g of triphenyl hexafluoroantimonate, stirring at a speed of 300rpm, stirring for 40min, to obtain HC slurry.
[0035] Step 22: Use a scraper to apply the HC slurry (speed 30 cm / min) on a 50 μm thick CPI film (purchased from Kolon, South Korea). Place the coated CPI film in an oven at 80°C and dry it for 25 min. Then, place the film under nitrogen at 1500 mJ / cm 2 After photocuring with a UV lamp with a radiation dose of 1.5 %, a HC-CPI film with a HC (hardened coating) thickness of 35 μm was obtained.
[0036] Example 3
[0037] In this embodiment, the composition ratio of each raw material of the formula slurry is as follows (by mass percentage):
[0038]
[0039] The specific preparation method is:
[0040] Step 31, add 70g of epoxycyclohexylethyl-trapezolic polysilsesquioxane to 25.5g of propylene glycol methyl ether acetate, stirring at a speed of 200rpm, stirring for 60min; add 3.5g of polypropylene glycol monomethyl ether (Mw=1k) at a stirring speed of 300rpm, stirring for 40min; add 1g of triphenyl hexafluoroantimonate, stirring at a speed of 300rpm, stirring for 40min, to obtain HC slurry.
[0041] Step 32: Use a scraper to apply the HC slurry (speed 30 cm / min) on a 50 μm thick CPI film (purchased from Kolon, South Korea). Place the coated CPI film in an oven at 80°C and dry it for 25 min. Then, place the film under nitrogen at 1200 mJ / cm 2 After photocuring with a UV lamp with a radiation dose of 1.5 %, a HC-CPI film with a HC (hardened coating) thickness of 35 μm was obtained.
[0042] Example 4
[0043] In this embodiment, the composition ratio of each raw material of the formula slurry is as follows (by mass percentage):
[0044]
[0045] The specific preparation method is:
[0046] Step 41, add 70g of epoxycyclohexylethyl-trapezolic polysilsesquioxane to 25.5g of propylene glycol methyl ether acetate, stirring at a speed of 200rpm, stirring for 60min; add 3.5g of polypropylene glycol diglycidyl ether (grade 227, Mw=1k) at a stirring speed of 300rpm, stirring for 40min; add 1g of triphenyl hexafluoroantimonate, stirring at a speed of 300rpm, stirring for 40min, to obtain HC slurry.
[0047] Step 42: The HC slurry was coated on a 50 μm thick CPI film (purchased from Kolon, South Korea) using a scraper (speed 30 cm / min). The coated CPI film was placed in an oven at 80°C and dried for 25 min. Then, the film was heated at 1200 mJ / cm 2 After photocuring with a UV lamp with a radiation dose of 1.5 %, a HC-CPI film with a HC (hardened coating) thickness of 35 μm was obtained.
[0048] The HC-CPI film prepared according to the ratio and preparation method in the above Examples 1 to 4 was tested for pencil hardness at break and HC elongation at break as well as the traditional POSS formula CPI film and LPSQ formula CPI film to verify the performance of the high-toughness epoxy polysilsesquioxane optical coating of the present invention.
[0049] Breaking pencil hardness test: Based on GB / T 6739-2006 standard, the test method is to apply a load of 750g through an automatic pencil hardness tester, use a Mitsubishi hardness pencil to move the pencil at a speed of 1mm / s, and test the pencil hardness of HC-CPI. When a scratch exceeding 3mm is found, the pencil hardness is reduced and the test is repeated. Finally, the maximum hardness that passes the test is recorded as the pencil hardness of the sample.
[0050] HC elongation at break test: The HC-CPI film was laser cut into strip samples of 10 mm × 150 mm. The distance between the upper and lower clamps of a universal testing machine was set to 60 mm. The strips were clamped on the clamps for tensile testing at a tensile rate of 0.5 mm / min. The HC surface was observed until cracks appeared and the test was stopped. The displacement S (unit: mm) was recorded. HC elongation at break = (S-60) / 60*100%.
[0051] The pencil hardness at break and the HC elongation at break of the HC-CPI film, the conventional POSS CPI film and the LPSQ CPI film were tested according to the above method. The results are shown in Table 1 below.
[0052] Table 1. Performance comparison of HC-CP prepared in Examples 1 to 4 and conventional CPI membranes
[0053]
[0054]
[0055] It can be seen from the data in Table 1 above that the HC-CPI film prepared by the method of the present invention has a higher elongation at break than the CPI film of the traditional formula at the same thickness, indicating that the present invention improves the toughness of the coating material while maintaining the original high strength, hardness, high thermal stability and other excellent properties of the CPI film by introducing long-chain flexible molecules between the polysilsesquioxane monomer molecules, and can be better used for folding screen cover protection.
[0056] It should be understood that the above description of the preferred embodiment is relatively detailed and cannot be regarded as limiting the scope of patent protection of the present invention. Under the enlightenment of the present invention, ordinary technicians in this field can also make substitutions or modifications without departing from the scope of protection of the claims of the present invention, which all fall within the scope of protection of the present invention. The scope of protection requested for the present invention shall be based on the attached claims.
Claims
1. A high-toughness epoxy polysilsesquioxane optical coating, characterized in that: The raw materials include epoxy polysilsesquioxane, a flexibilizer and a toughener, a photoinitiator and a solvent.
2. The high-toughness epoxy polysilsesquioxane optical coating according to claim 1, characterized in that: The epoxy-containing polysilsesquioxane is a cage-shaped polysilsesquioxane POSS or a ladder-shaped polysilsesquioxane LPSQ or a random polysilsesquioxane; the epoxy functional group includes epoxy cyclohexyl and glycidyl ether oxypropyl, and the epoxy functional group is a bifunctional group or a multifunctional group.
3. The high-toughness epoxy polysilsesquioxane optical coating according to claim 1, characterized in that: The photoinitiator is at least one of an onium salt initiator, a metal organic initiator, and an organosilane initiator; the solvent is at least one of 2-butanone, ethyl acetate, and propylene glycol methyl ether acetate.
4. The high-toughness epoxy polysilsesquioxane optical coating according to claim 1, characterized in that: The flexibility and toughening agent is one or more of mono / bi-terminal epoxy polyether silicone oil (Mw≤2k), mono / bi-terminal epoxy polyether (Mw≤3k), mono / bi-terminal hydroxyl polyether silicone oil (Mw≤2k), mono / bi-terminal hydroxyl-terminated polyether (Mw≤3k), ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and pentaerythritol tetraglycidyl ether.
5. The high-toughness epoxy polysilsesquioxane optical coating according to claim 1, characterized in that: The total mass proportion of each raw material is: epoxy polysilsesquioxane 40~85 wt%, solvent 10~50 wt%, flexibility and toughening agent 0.5~15 wt%, photoinitiator 0.5~2 wt%.
6. A method for preparing a high-toughness epoxy polysilsesquioxane optical coating as claimed in claims 1-5, characterized in that: The following steps are involved: Step 1, adding epoxy polysilsesquioxane, a flexibilizer and a photoinitiator to a solvent in sequence, stirring continuously until uniform, to obtain a formula slurry; Step 2: coating the obtained formula slurry on the surface of the substrate, and then drying the solvent and UV curing, so as to form an optical coating with both hardness and toughness on the surface of the substrate.
7. The method for preparing a high-toughness epoxy polysilsesquioxane optical coating according to claim 6, characterized in that: The stirring speed in step 1 is 200-300 rpm. After the epoxy polysilsesquioxane is added to the solvent and stirred for 30-60 minutes, the softening and toughening agent is added and stirred for 40-50 minutes, and finally the photoinitiator is added and stirred for 30-60 minutes until the solution is uniformly stirred to obtain a formula slurry.
8. The method for preparing a high-toughness epoxy polysilsesquioxane optical coating according to claim 6, characterized in that: The coating method in step 2 is any one of roller coating, blade coating, dip coating, wheel coating, spin coating, and slit coating.
9. The method for preparing a high-toughness epoxy polysilsesquioxane optical coating according to claim 6, characterized in that: The drying temperature in step 2 is 60-110°C, the drying time is 20-90 min, and the radiation dose of the UV curing is 700-2000 mJ / cm 2 .
10. The method for preparing a high-toughness epoxy polysilsesquioxane optical coating according to claim 6, characterized in that: The substrate in step 2 is at least one of a CPI substrate, a PET substrate, and polymethyl methacrylate (PMMA).
Citation Information
Patent Citations
High-strength, flexible, transparent, wear-resistant, and hardening coating on foldable screen surface and its preparation method
CN111454648B
Low-shrinkage, high-hardness, flexible and anti-fingerprint hardened coating and preparation method thereof
CN114539915A
A mobile phone glass back cover coating liquid, its preparation method and application
CN114702900B
Building structure adhesive and preparation method thereof
CN112029462A
Alicyclic epoxy resin injection material for composite insulator low-temperature-resistant hard sheath and preparation method thereof
CN112980148A
Cited By
Transparent multifunctional material as well as preparation method and application thereof
CN120005116A