High-strength low-carbon-residue two-component binder as well as preparation method and application thereof

By using a two-component binder system in the binder jet forming process, combining low molecular weight and high molecular weight polymers, and optimizing solvents and surfactants, the inadequate body strength of the aqueous binder and high carbon residues are solved. The problem is that high mechanical strength and low carbon residue effects are achieved.

CN118909571AActive Publication Date: 2024-11-08UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202410968069.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The existing water-based adhesives have insufficient body strength and high residual carbon content in the adhesive spray forming process, making it difficult to take into account both mechanical properties and impurity control.

Method used

A two-component binder system is adopted that combines low-molecular and high-molecular-weight polymers and optimizes solvent and surfactant ratios and interactions to provide high mechanical strength and reduce carbon residue.

Benefits of technology

The mechanical strength of the blank is significantly improved and carbon residue is reduced. The bending strength exceeds 10MPa and the carbon content is less than 0.2 wt.%, which improves the quality and performance of additive manufacturing products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909571A_ABST
    Figure CN118909571A_ABST
Patent Text Reader

Abstract

The invention relates to the field of additive manufacturing, and provides a high-strength low-carbon-residue two-component binder and a preparation method and application thereof.The two-component binder comprises a first component, a second component, a solvent and a surfactant, the first component is composed of a low-molecular-weight polymer, and the weight-average molecular weight ranges from 2000 to 20000; the second component is composed of a high-molecular-weight polymer, and the weight-average molecular weight of the second component ranges from 50000 to 500000; the low-molecular-weight polymer provides structural support in the initial stage of printing and spraying a green body; the high-molecular-weight polymer is used for improving the strength of the green body and reducing the impurity content in the heat treatment process. By optimizing the combination and proportion of the low-molecular-weight polymer and the high-molecular-weight polymer, the mechanical strength of the green body is remarkably improved, and impurity residues, especially carbon residues, of the green body are reduced. The finally prepared green body has excellent mechanical strength after being dried, the impurity content is extremely low, and the quality and performance of an additive manufacturing product are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of additive manufacturing, and in particular to a high-strength and low-carbon residual two-component binder, a preparation method and an application thereof. Background Art

[0002] Additive Manufacturing (AM) has received extensive attention and application in recent years, especially in the manufacturing field with high complexity, high precision and high customization requirements. Among them, Binder Jetting (BJ), as an important process of additive manufacturing, has gradually become one of the important technologies in industrial production with its advantages of high speed, high efficiency and variety of material selection.

[0003] In the binder jet forming process, the powder material is bonded layer by layer by spraying liquid binder to finally form a complex three-dimensional structure. In the existing binder jet forming process, water-based binders have been widely used due to their environmental protection and safety advantages. However, there are still some problems that need to be solved in the practical application of water-based binders: First, the blank prepared using water-based binders usually cannot achieve sufficient mechanical strength after curing, which makes it easy to break during subsequent processing and use. Secondly, water-based binders will leave a lot of impurities, especially carbon residues, during the curing process, which affects the performance and quality of the final product. In order to improve the overall performance of the binder jet forming process, it has become a technical problem to be solved to develop a two-component binder system that can provide high mechanical strength while significantly reducing the residual carbon content.

[0004] Traditional binder systems mainly rely on single-component polymers, which makes it difficult to achieve an ideal balance between mechanical properties and impurity control. To this end, researchers have begun to try to use a combination of multiple polymers in order to improve the overall performance of the binder through the synergistic effect of polymers with different molecular weights and functions.

[0005] In this context, the present invention proposes a two-component binder system, which includes a combination of a low molecular weight polymer and a high molecular weight polymer, and optimizes the ratio and interaction between the two, in order to significantly reduce the carbon residue of the green body while maintaining high mechanical strength. In addition, the present invention also optimizes the solvent and surfactant in the binder system to further improve the performance of the binder and the spray forming effect. Summary of the invention

[0006] The purpose of the present invention is to overcome at least one of the deficiencies of the prior art and to provide a high-strength, low-carbon residual two-component binder, a preparation method and an application thereof, aiming to solve the technical problems of insufficient green body strength and high impurity residue faced by existing water-based binders in the binder injection molding process.

[0007] The present invention adopts the following technical solution:

[0008] On the one hand, the present invention provides a high-strength and low-carbon residue two-component binder, the two-component binder is used for binder injection molding of additive manufacturing, and the two-component binder includes a first component, a second component, a solvent and a surfactant:

[0009] The first component is composed of a low molecular weight polymer, and the weight average molecular weight of the low molecular weight polymer is in the range of 2000-20000;

[0010] The second component is composed of a high molecular weight polymer, and the weight average molecular weight of the high molecular weight polymer is in the range of 50,000-500,000;

[0011] The low molecular weight polymer provides structural support in the initial stage of printing and jetting the blank; the high molecular weight polymer is used to improve the strength of the blank and reduce the impurity content during the heat treatment process; the solvent is used to dissolve the first component and the second component to form a mixed solution; the surfactant stabilizes the mixed solution system and changes the rheological properties of the two-component adhesive so that the two-component adhesive can be stably sprayed out from the nozzle.

[0012] As for any possible implementation described above, an implementation is further provided, wherein the low molecular weight polymer includes one or more combinations of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP) and polyethyleneimine (PEI).

[0013] Any possible implementation as described above further provides an implementation, wherein the high molecular weight polymer includes one or a combination of water-based acrylic resin, water-based epoxy resin and water-based polyurethane.

[0014] Any possible implementation as described above further provides an implementation, wherein the mass ratio of the low molecular weight polymer to the high molecular weight polymer is 5:1 to 1:1.

[0015] Any possible implementation as described above further provides an implementation, wherein the solid content of the waterborne acrylic resin, waterborne epoxy resin and waterborne polyurethane is 30-70 wt. %. The above-mentioned resins are in the form of emulsion, and the solid content is the polymer content in the emulsion.

[0016] The low molecular weight polymer selected by the present invention begins to thermally decompose at a relatively low temperature, which is manifested as the first obvious platform or mass loss stage on the TGA curve. In addition, the low molecular weight polymer helps to reduce the friction between materials during the printing process. At this stage, the low molecular weight polymer will decompose rapidly, forming a polymer channel and releasing volatile products. Due to the high proportion of low molecular weight polymers, the low molecular weight polymers have been decomposed during the drying and curing process, which greatly reduces the impurity content of the blank, especially the carbon content.

[0017] The high molecular weight polymer used in the present invention has high thermal stability due to its long chain structure and usually begins to decompose at a higher temperature. During the drying and curing process, the high molecular weight polymer does not decompose, and the larger molecular weight ensures the high strength of the blank. In addition, the high molecular weight polymer accounts for a relatively low proportion in the binder system and will not introduce excess impurities.

[0018] Adapting the two-component binder to a suitable debinding process ensures a low impurity content in the product.

[0019] Any possible implementation as described above further provides an implementation, wherein the solvent includes but is not limited to one or more combinations of ethylene glycol methyl ether, propylene glycol methyl ether, ethylene glycol, glycerol and triethylene glycol, and the proportion of the solvent is 60 to 90 wt.% of the two-component adhesive.

[0020] Any possible implementation as described above further provides an implementation, wherein the surfactant includes but is not limited to one or more combinations of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, alkyl mannose and silicone surfactants, and the proportion of the surfactant is 0.1 to 1.0 wt.% of the two-component binder.

[0021] The solvent and surfactant selected in the present invention are mainly considered to be compatible with the system, and no precipitate or flocculent is generated.

[0022] On the other hand, Figure 1 As shown, the present invention also provides a method for preparing the above-mentioned high-strength and low-carbon residue two-component binder, characterized in that the method comprises:

[0023] S1, preparing a first component solution: dissolving a low molecular weight polymer in a solvent to obtain a first component solution;

[0024] S2, preparing a second component solution: dissolving a high molecular weight polymer in a solvent to obtain a second component solution;

[0025] S3, mixing the first component solution and the second component solution according to a predetermined mass ratio, and stirring evenly to obtain a mixed solution;

[0026] S4, adding a predetermined amount of surfactant to the mixed solution, stirring it sufficiently to make it uniformly dispersed, and obtaining the two-component adhesive.

[0027] Any possible implementation as described above further provides an implementation, in step S1, the concentration of the first component solution is 5-20wt.%; in step S2, the concentration of the second component solution is 1%-20wt.%.

[0028] On the other hand, the present invention also provides an application of the above-mentioned high-strength and low-carbon residue two-component binder, wherein the two-component binder is applied to a binder spray forming green body process, specifically comprising:

[0029] The two-component binder is sprayed onto a substrate through a spray forming process to obtain a green body, and the green body is heated to solidify to obtain a high-strength and low-carbon residue green body;

[0030] The green body has a flexural strength of >10 MPa and a carbon content of <0.2 wt.% after solidification.

[0031] The conventional binder generally produces a blank with a flexural strength of less than 11 MPa and a residual carbon content of more than 0.8 wt.%. When the blank strength is more than 10 MPa, the residual carbon content is more than 1.5 wt.%.

[0032] The beneficial effects of the present invention are:

[0033] The present invention significantly improves the mechanical strength of the green body and reduces the impurity residue, especially carbon residue, of the green body by optimizing the combination and ratio of low molecular weight and high molecular weight polymers. The green body finally prepared has excellent mechanical strength (flexural strength>10MPa) and extremely low impurity content (carbon content<0.2wt.%) after drying, which greatly improves the quality and performance of additive manufacturing products. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The figure is a schematic flow chart of a method for preparing a high-strength and low-carbon-residue dual-component binder according to an embodiment of the present invention. DETAILED DESCRIPTION

[0035] The specific embodiments of the present invention will be described in detail below in conjunction with specific embodiments. It should be noted that the technical features or combinations of technical features described in the following embodiments should not be considered isolated, and they can be combined with each other to achieve better technical effects.

[0036] The embodiment of the present invention provides a high-strength and low-carbon residue two-component binder for binder injection molding in additive manufacturing. The two-component binder includes a first component, a second component, a solvent and a surfactant:

[0037] The first component is composed of a low molecular weight polymer, and the weight average molecular weight of the low molecular weight polymer is in the range of 2000-20000;

[0038] The second component is composed of a high molecular weight polymer, and the weight average molecular weight of the high molecular weight polymer is in the range of 50,000-500,000;

[0039] The low molecular weight polymer provides structural support in the initial stage of printing and jetting the blank; the high molecular weight polymer is used to improve the strength of the blank and reduce the impurity content during the heat treatment process; the solvent is used to dissolve the first component and the second component to form a mixed solution; the surfactant stabilizes the mixed solution system and changes the rheological properties of the two-component adhesive so that the two-component adhesive can be stably sprayed out from the nozzle.

[0040] In a specific embodiment, the low molecular weight polymer includes one or more combinations of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP) and polyethyleneimine (PEI).

[0041] In a specific embodiment, the high molecular weight polymer includes one or a combination of waterborne acrylic resin, waterborne epoxy resin and waterborne polyurethane.

[0042] In a specific embodiment, the mass ratio of the low molecular weight polymer to the high molecular weight polymer is 5:1 to 1:1.

[0043] In a specific embodiment, the solid content of the waterborne acrylic resin, waterborne epoxy resin and waterborne polyurethane is 30-70 wt.%.

[0044] In a specific embodiment, the solvent includes one or more combinations of ethylene glycol methyl ether, propylene glycol methyl ether, ethylene glycol, glycerol and triethylene glycol, and the proportion of the solvent is 60 to 90 wt.% of the two-component binder.

[0045] In a specific embodiment, the surfactant is one or more combinations of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, alkyl mannose and silicone surfactants, and the proportion of the surfactant is 0.1-1.0 wt.% of the two-component binder.

[0046] like Figure 1 As shown, a method for preparing the above-mentioned high-strength and low-carbon-residue two-component binder according to an embodiment of the present invention comprises:

[0047] S1, preparing a first component solution: dissolving a low molecular weight polymer in a solvent to obtain a first component solution;

[0048] S2, preparing a second component solution: dissolving a high molecular weight polymer in a solvent to obtain a second component solution;

[0049] S3, mixing the first component solution and the second component solution according to a predetermined mass ratio, and stirring evenly to obtain a mixed solution;

[0050] S4, adding a predetermined amount of surfactant to the mixed solution, stirring it sufficiently to make it uniformly dispersed, and obtaining the two-component adhesive.

[0051] In a specific embodiment, in step S1, the concentration of the first component solution is 5-20 wt. %; in step S2, the concentration of the second component solution is 1%-20 wt. %.

[0052] An embodiment of the present invention provides an application of the above-mentioned high-strength and low-carbon residue two-component binder, wherein the two-component binder is applied to a binder spray forming green body process, specifically comprising:

[0053] The two-component binder is sprayed onto a substrate through a spray forming process to obtain a green body, and the green body is heated to solidify to obtain a high-strength and low-carbon residue green body;

[0054] The green body has a flexural strength of >10 MPa and a carbon content of <0.2 wt.% after solidification.

[0055] Example 1

[0056] The specific process of preparing the embryo body using the high-strength and low-carbon residue dual-component binder of the present invention is as follows:

[0057] (1) Material preparation:

[0058] Low molecular weight polymer: polyvinyl alcohol (PVA), weight average molecular weight is 1000;

[0059] High molecular weight polymer: water-based acrylic resin, weight average molecular weight of 150,000;

[0060] Solvent: mixture of ethylene glycol methyl ether and propylene glycol methyl ether, ratio 1:1;

[0061] Surfactant: sodium dodecylbenzene sulfonate;

[0062] (2) Preparation of the first component solution

[0063] Dissolving PVA in a mixed solvent of ethylene glycol methyl ether and propylene glycol methyl ether to obtain a first component solution with a concentration of 10 wt.%;

[0064] (3) Preparation of the second component solution

[0065] Dissolving an aqueous acrylic resin in a mixed solvent of ethylene glycol methyl ether and propylene glycol methyl ether to obtain a second component solution with a concentration of 5 wt.%;

[0066] (4) Configure a two-component binder

[0067] The first component solution and the second component solution are mixed in a mass ratio of 2:1, and stirred evenly to form a two-component adhesive;

[0068] (5) Adding surfactant

[0069] Add 0.5 wt.% of sodium dodecylbenzene sulfonate to the two-component binder and stir thoroughly to make it evenly dispersed in the binder;

[0070] (6) Spray Forming

[0071] The prepared two-component binder is loaded into a binder jet printer and sprayed onto the pre-laid stainless steel 316L powder substrate through a nozzle; during the spraying process, the movement path and spraying frequency of the nozzle are controlled to ensure that the binder is evenly distributed on the powder bed;

[0072] (7) Heating and curing

[0073] Move the powder bed into an oven set at 180°C and set the curing time at 120 min;

[0074] (8) Green body performance test

[0075] The flexural strength test and carbon content analysis were performed on the solidified green body. The test results showed that the flexural strength of the green body was 12 MPa and the carbon content was 0.10 wt.%, which met the design objectives of the present invention.

[0076] Example 2

[0077] The specific process of preparing the embryo body using the high-strength and low-carbon residue dual-component binder of the present invention is as follows:

[0078] (1) Material preparation

[0079] Low molecular weight polymer: polyvinylpyrrolidone (PVP), weight average molecular weight of 15000;

[0080] High molecular weight polymer: water-based epoxy resin, weight average molecular weight of 200,000;

[0081] Solvent: mixture of glycerol and ethylene glycol in a ratio of 1:1;

[0082] Surfactant: sodium lauryl sulfate;

[0083] (2) Preparation of the first component solution

[0084] dissolving a water-based epoxy resin in a mixed solvent of glycerol and ethylene glycol to obtain a second component solution having a concentration of 5 wt.%;

[0085] (3) Preparation of the second component solution

[0086] Dissolving an aqueous acrylic resin in a mixed solvent of ethylene glycol methyl ether and propylene glycol methyl ether to obtain a second component solution with a concentration of 5 wt.%;

[0087] (4) Configure a two-component binder

[0088] The first component solution and the second component solution are mixed in a mass ratio of 3:1, and stirred evenly to form a multi-component adhesive;

[0089] (5) Adding surfactant

[0090] Add 0.3 wt.% of sodium dodecyl sulfate to the two-component binder and stir thoroughly to make it evenly dispersed in the binder;

[0091] (6) Spray Forming

[0092] The prepared multi-component binder is loaded into a binder jet printer and sprayed onto the pre-laid 17-4PH powder substrate through a nozzle; during the spraying process, the movement path and spraying frequency of the nozzle are controlled to ensure that the binder is evenly distributed on the powder bed;

[0093] (7) Heating and curing

[0094] Move the powder bed into an oven set at 200°C and set the curing time at 120 min;

[0095] (8) Green body performance test

[0096] The flexural strength test and carbon content analysis were performed on the solidified green body. The test results showed that the flexural strength of the green body was 15 MPa and the carbon content was 0.17 wt.%, which met the design objectives of the present invention.

[0097] Example 3

[0098] The specific process of preparing the embryo body using the high-strength and low-carbon residue dual-component binder of the present invention is as follows:

[0099] (1) Material preparation

[0100] Low molecular weight polymer: polyethyleneimine (PEI), weight average molecular weight of 8000;

[0101] High molecular weight polymer: waterborne polyurethane, weight average molecular weight is 250000;

[0102] Solvent: mixture of propylene glycol methyl ether and triethylene glycol, ratio 2:1;

[0103] Surfactant: Alkyl mannose;

[0104] (2) Preparation of the first component solution

[0105] Dissolving PEI in a mixed solvent of propylene glycol methyl ether and triethylene glycol to obtain a first component solution with a concentration of 12 wt.%;

[0106] (3) Preparation of the second component solution

[0107] Dissolving waterborne polyurethane in a mixed solvent of propylene glycol methyl ether and triethylene glycol to obtain a second component solution with a concentration of 8 wt.%;

[0108] (4) Configure a two-component binder

[0109] The first component solution and the second component solution are mixed in a mass ratio of 1:1, and stirred evenly to form a multi-component adhesive;

[0110] (5) Adding surfactant

[0111] Add 0.2 wt.% of alkyl glycosides to the multi-component binder and stir thoroughly to make it evenly dispersed in the binder;

[0112] (6) Spray Forming

[0113] The prepared multi-component binder is loaded into a binder jet printer and sprayed onto the pre-laid H13 powder substrate through a nozzle; during the spraying process, the movement path and spraying frequency of the nozzle are controlled to ensure that the binder is evenly distributed on the powder bed;

[0114] (7) Heating and curing

[0115] Move the powder bed to an oven set at 180°C and set the curing time at 150 min;

[0116] (8) Green body performance test

[0117] The flexural strength test and carbon content analysis were performed on the solidified green body. The test results showed that the flexural strength of the green body was 13 MPa and the carbon content was 0.08 wt.%, which met the design objectives of the present invention.

[0118] Through the specific operations and test results of the above three embodiments, it can be seen that the two-component adhesive of the present invention can achieve the performance goals of high mechanical strength and low impurity residue under different conditions, and has broad application prospects.

[0119] Although several embodiments of the present invention have been given herein, those skilled in the art should understand that the embodiments of the present invention may be modified without departing from the spirit of the present invention. The above embodiments are merely exemplary and should not be used as a limitation on the scope of the present invention.

Claims

1. A high-strength, low-carbon-residue two-component binder, characterized in that: The two-component binder is used for binder injection molding of additive manufacturing, and the two-component binder includes a first component, a second component, a solvent and a surfactant: The first component is composed of a low molecular weight polymer, and the weight average molecular weight of the low molecular weight polymer is in the range of 2000-20000; The second component is composed of a high molecular weight polymer, and the weight average molecular weight of the high molecular weight polymer is in the range of 50,000-500,000; The low molecular weight polymer provides structural support in the initial stage of printing and jetting the blank; the high molecular weight polymer is used to improve the strength of the blank and reduce the impurity content during the heat treatment process; the solvent is used to dissolve the first component and the second component to form a mixed solution; the surfactant stabilizes the mixed solution system and changes the rheological properties of the two-component adhesive so that the two-component adhesive can be stably sprayed out from the nozzle.

2. The high-strength, low-carbon-residue two-component binder according to claim 1, characterized in that: The low molecular weight polymer includes one or more combinations of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP) and polyethyleneimine (PEI).

3. The high-strength, low-carbon-residue two-component binder according to claim 1, characterized in that: The high molecular weight polymer includes one or more combinations of waterborne acrylic resin, waterborne epoxy resin and waterborne polyurethane.

4. The high-strength, low-carbon-residue two-component binder according to claim 1, characterized in that: The mass ratio of the low molecular weight polymer to the high molecular weight polymer is 5:1 to 1:

1.

5. The high-strength, low-carbon-residue two-component binder according to claim 3, characterized in that: The solid content of the waterborne acrylic resin, waterborne epoxy resin and waterborne polyurethane is 30-70 wt.%.

6. The high-strength, low-carbon-residue two-component binder according to claim 1, characterized in that: The solvent comprises one or more combinations of ethylene glycol methyl ether, propylene glycol methyl ether, ethylene glycol, glycerol and triethylene glycol, and the proportion of the solvent is 60-90 wt.% of the two-component adhesive.

7. The high-strength, low-carbon-residue two-component binder according to claim 1, characterized in that: The surfactant comprises one or more combinations of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, alkyl glycosides and silicone surfactants, and the proportion of the surfactant is 0.1-1.0 wt.% of the two-component binder.

8. A method for preparing a high-strength, low-carbon-residue dual-component binder according to any one of claims 1 to 7, characterized in that: The method comprises: S1, preparing a first component solution: dissolving a low molecular weight polymer in a solvent to obtain a first component solution; S2, preparing a second component solution: dissolving a high molecular weight polymer in a solvent to obtain a second component solution; S3, mixing the first component solution and the second component solution according to a predetermined mass ratio, and stirring evenly to obtain a mixed solution; S4, adding a predetermined amount of surfactant to the mixed solution, stirring it sufficiently to make it uniformly dispersed, and obtaining the two-component adhesive.

9. The method for preparing a high-strength and low-carbon-residue two-component binder according to claim 8, characterized in that: In step S1, the concentration of the first component solution is 5-20 wt. %; in step S2, the concentration of the second component solution is 1%-20 wt. %.

10. An application of the high-strength and low-carbon-residue two-component binder according to any one of claims 1 to 7, characterized in that: The two-component binder is applied to the binder spray forming green body process, specifically comprising: The two-component binder is sprayed onto a substrate through a spray forming process to obtain a green body, and the green body is heated to solidify to obtain a high-strength and low-carbon residue green body; The green body has a flexural strength of >10 MPa and a carbon content of <0.2 wt.% after solidification.

Citation Information

Patent Citations

  • Material systems for additive manufacturing

    CN110312582A

  • Thermoplastic binders for use in binder jetting additive manufacturing

    CN110997284A

  • Binder for powder injection molding

    CN115108840A

  • Thermal excitation free radical polymerization binder for binder jet 3D printing and preparation method of thermal excitation free radical polymerization binder

    CN117264574A

  • Water-based binder solutions for additive manufacturing processes

    CN117467376A

Cited By

  • Binder jetting composition

    GB2705916A