Bi-component polyurethane heat-conducting structural adhesive and preparation method thereof

By using two-component structure and aluminum hydroxide filler in polyurethane thermally conductive structural adhesives, the thermal conductivity network is formed, which solves the problems of high density, poor toughness and insufficient flame retardant performance, and achieves high thermal conductivity, low density, good toughness and flame retardant. Combination of performance.

CN118909584APending Publication Date: 2024-11-08TECHSTORM MATERIAL TECH SHANGHAI CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310502479.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

While improving thermal conductivity, the existing polyurethane thermally conductive structural adhesives lead to increased density, reduced flexibility, easy to break, and difficult to achieve the flame retardant performance of UL94-V0 at low thickness.

Method used

Two-component polyurethane thermally conductive structural adhesive is used, and a thermal conductivity network is formed to improve toughness and Thermal conductivity, while reducing product density under the premise of the same thermal conductivity.

Benefits of technology

It realizes the flame retardant performance of UL94-V0 while maintaining thermal conductivity while reducing the density of polyurethane products, improving toughness, avoiding fractures, and achieving the flame retardant performance of UL94-V0 at lower thicknesses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004214291200000111
    Figure BDA0004214291200000111
Patent Text Reader

Abstract

The invention provides a two-component polyurethane heat-conducting structural adhesive and a preparation method thereof, and relates to the technical field of polyurethane heat-conducting structural adhesives. The polyurethane heat-conducting structural adhesive comprises a component A and a component B in a volume ratio of 1: (0.9-1.1), the component A comprises a polyol composition and a first heat-conducting filler in a weight ratio of 1: (1-2); the polyol composition comprises polyether polyol and castor oil modified polyol in a weight ratio of 1: (1-3); the component B comprises a prepolymer and a second heat-conducting filler in a weight ratio of 3: (7-12); the first heat-conducting filler and the second heat-conducting filler both comprise aluminum hydroxide; and the component B also comprises 0.3-0.8 wt% of a viscosity reduction auxiliary agent. On the premise that the same heat conductivity coefficient is achieved, the density of the polyurethane adhesive can be reduced, the toughness can be improved, and the flame retardant property of UL94-V0 can be achieved under the condition that the thickness is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane thermal conductive structural adhesive, and in particular to a two-component polyurethane thermal conductive structural adhesive and a preparation method thereof. Background Art

[0002] As domestic policies vigorously develop new energy, new energy vehicles, wind power, and photovoltaic energy storage industries are booming, and all three industries require batteries to be placed and fixed in a large battery pack to form a battery pack for discharge or energy storage applications. In order to meet the current requirements for high power output, high energy storage performance, and low density and light weight of batteries, the requirements for battery thermal conductivity and bonding are becoming increasingly higher. Currently, thermal conductive structural adhesives are often used to conduct heat and bond batteries.

[0003] At present, the polyurethane thermal conductive structural adhesive commonly used in batteries mostly uses alumina as the main thermal conductive filler, and the density of alumina is 3.95g / cm 3 The cured product of polyurethane resin is generally 1.05-1.1g / cm 3 If calculated according to the thermal conductivity requirement of 1.2w, the final amount of alumina added needs to account for about 60% of the overall mass of the thermal conductive structural adhesive, and the density of the final product is generally 1.8-2.0g / cm 3 The product has a high density, which is not conducive to the lightweight design of the battery. In addition, adding a large amount of thermal conductive filler to the polyurethane thermal conductive structural adhesive will directly lead to a decrease in the flexibility of the product, an increase in rigidity, and an increase in hardness, making the product more prone to breakage.

[0004] Therefore, there is an urgent need to provide a two-component polyurethane thermal conductive structural adhesive to improve the problems existing in the above-mentioned prior art. Summary of the invention

[0005] The purpose of the present invention is to provide a two-component polyurethane thermal conductive structural adhesive and a preparation method thereof, which can reduce the density of the polyurethane thermal conductive structural adhesive product while achieving the same thermal conductivity coefficient, and improve the toughness of the product so that the product is not easy to break, and can achieve UL94-V0 flame retardant performance at a lower thickness.

[0006] In a first aspect, the present invention provides a two-component polyurethane thermal conductive structural adhesive, which adopts the following technical solution:

[0007] It includes component A and component B in a volume ratio of 1:(0.9-1.1);

[0008] The A component includes a polyol composition and a first thermally conductive filler in a weight ratio of 1:(1-2);

[0009] Wherein, the polyol composition comprises polyether polyol and castor oil modified polyol in a weight ratio of 1:(1-3);

[0010] The B component includes a prepolymer and a second thermally conductive filler in a weight ratio of 3:(7-12);

[0011] The first thermally conductive filler and the second thermally conductive filler are both aluminum hydroxide;

[0012] The B component also includes 0.3-0.8 wt % of a viscosity reducing agent.

[0013] The two-component polyurethane thermally conductive structural adhesive provided by the present invention has the following beneficial effects: a first thermally conductive filler and a second thermally conductive filler are added to component A and component B, and both the first thermally conductive filler and the second thermally conductive filler are aluminum hydroxide, so that while improving the overall thermal conductivity of the thermally conductive structural adhesive, it is possible to reduce the density of the polyurethane thermally conductive structural adhesive product under the premise of the same thermal conductivity coefficient, and adding a viscosity reducing agent to component B can help distribute the aluminum hydroxide in the thermally conductive structural adhesive, so that the aluminum hydroxide is evenly distributed in the thermally conductive structural adhesive, which can improve the product toughness of the polyurethane thermally conductive structural adhesive and improve the overall thermal conductivity, so that the polyurethane thermally conductive structural adhesive maintains high thermal conductivity after use, is not prone to breakage, and can achieve UL94-V0 flame retardancy at a relatively low thickness.

[0014] Optionally, the viscosity reducing agent is one or more combinations of phosphate esters and high molecular weight copolymer alkyl ammonium salts.

[0015] Optionally, the high molecular weight copolymer alkyl ammonium salt is a mixture of a reaction product of a special polymer and 2-ethylhexyl 2-acrylate, and a polyethylene polypropylene glycol monobutyl ether phosphate compound; wherein the special polymer is a polymer of ethylenediamine and ethyleneimine.

[0016] Optionally, the first thermally conductive filler and the second thermally conductive filler both include aluminum hydroxide of two different particle sizes.

[0017] Optionally, the first thermally conductive filler includes a first small-particle aluminum hydroxide and a first large-particle aluminum hydroxide, and the weight ratio of the first small-particle aluminum hydroxide to the first large-particle aluminum hydroxide is 1:(1-5); the second thermally conductive filler includes a second small-particle aluminum hydroxide and a second large-particle aluminum hydroxide, and the weight ratio of the second small-particle aluminum hydroxide to the second large-particle aluminum hydroxide is 1:(1-5); the particle sizes of the first small-particle aluminum hydroxide and the second small-particle aluminum hydroxide are both ≤15μm; the particle sizes of the first large-particle aluminum hydroxide and the second large-particle aluminum hydroxide are both ≥20μm and ≤50μm. It is possible to improve the filling performance of aluminum hydroxides of different particle sizes in polyurethane products while maintaining the thermal conductivity and flame retardancy of polyurethane products, so that aluminum hydroxides of different particle sizes form a thermal conductive network in polyurethane products, and also improve the toughness of polyurethane products.

[0018] Optionally, the particle size of the first small-particle aluminum hydroxide is 5μm or 8μm; the particle size of the second small-particle aluminum hydroxide is 5μm or 8μm; the particle size of the first large-particle aluminum hydroxide is 20μm or 50μm; the particle size of the second large-particle aluminum hydroxide is 20μm or 50μm.

[0019] Optionally, the weight ratio of the polyol composition to the first thermally conductive filler is 7:(10-14).

[0020] Optionally, the weight ratio of the polyether polyol to the castor oil modified polyol is 1:3.

[0021] Optionally, the number average molecular weight of the polyether polyol is 500-2000 and the functionality is 3. The elongation at break of the product can be increased at the same strength, thereby ensuring that the thermal conductive structural adhesive has a certain toughness and strength after bonding, and ensuring that the thermal conductive structural adhesive product does not crack.

[0022] Optionally, the prepolymer is formed by prepolymerization of isocyanate and castor oil modified polyol, wherein the weight ratio of the isocyanate to the castor oil modified polyol is 10:(2-4).

[0023] Optionally, the preparation method of the prepolymer is: placing the isocyanate and the castor oil-modified polyol at 50-80° C. and reacting for 1-3 hours to obtain the prepolymer.

[0024] Optionally, the weight ratio of the isocyanate to the castor oil modified polyol is 10:2.75.

[0025] Optionally, the isocyanate includes one of CDMDI-100L, MDI-50 and MDI-100 produced by Wanhua Chemical Group Co., Ltd.

[0026] Optionally, the modified castor oil includes one or a combination of aliphatic modified castor oil polyol and aromatic modified castor oil polyol.

[0027] Optionally, the modified castor oil is selected from one or more combinations of H-30, H-31, H-52, H-368, AC-008, AC-009 produced by Ito Oil Manufacturing Co., Ltd., A-21, A-4100 produced by Shanghai Jingri New Material Technology Co., Ltd., and BP-09, BP-19 produced by Shanghai Benyou New Material Technology Co., Ltd.

[0028] Optionally, the castor oil-modified polyol includes one or a combination of aliphatic-modified castor oil polyol and aromatic-modified castor oil polyol.

[0029] Optionally, the castor oil modified polyol is selected from one or more combinations of H-30, H-31, H-52, H-368, AC-008, AC-009 produced by Ito Oil Manufacturing Co., Ltd., A-21, A-4100 produced by Shanghai Jingri New Material Technology Co., Ltd., and BP-09, BP-19 produced by Shanghai Benyou New Material Technology Co., Ltd.

[0030] In a second aspect, the present invention provides a method for preparing a two-component polyurethane thermally conductive structural adhesive, which adopts the following technical scheme and comprises the following steps:

[0031] preparing the A component;

[0032] preparing the B component;

[0033] The A component and the B component are mixed in a volume ratio of 1:(0.9-1.1). DETAILED DESCRIPTION

[0034] The present application is further described in detail below with reference to embodiments.

[0035] Example

[0036] Example 1

[0037] A two-component polyurethane thermal conductive structural adhesive, the preparation steps of which include:

[0038] S1. Preparation of component A:

[0039] In parts by weight, 100 parts of polyether polyol (purchased from Shandong Bluestar Dongda Chemical Co., Ltd., brand MN-1000, molecular weight 1000, functionality 3) and 100 parts of castor oil modified polyol (purchased from Ito Oil Products Co., Ltd., brand H-368, aromatic castor oil modified polyol) were uniformly mixed in a weight ratio of 1:1 to prepare a polyol composition; aluminum hydroxide with an average particle size of 8 μm and aluminum hydroxide with an average particle size of 20 μm were selected and mixed in a weight ratio of 1:1 as the first thermal conductive filler;

[0040] 100 parts by weight of the polyol composition and 100 parts by weight of the first thermally conductive filler are placed in a vacuum environment, the weight ratio of the polyol composition to the first thermally conductive filler being 1:1, and stirred at room temperature until the mixture is uniformly mixed, to obtain component A;

[0041] S2. Preparation of component B:

[0042] In parts by weight, 100 parts of isocyanate (purchased from Wanhua Chemical Group Co., Ltd., brand CDMDI-100L) and 30 parts of modified castor oil (Ito Oil Products Co., Ltd., H-368) were uniformly mixed in a weight ratio of 10:3, placed in an environment of 60°C for reaction for 2 hours, and a prepolymer was obtained; aluminum hydroxide with an average particle size of 5 μm and aluminum hydroxide with an average particle size of 50 μm were selected as the second thermal conductive filler after being mixed in a weight ratio of 2:3;

[0043] In parts by weight, 30 parts of prepolymer, 70 parts of the second thermal conductive filler and 0.6 parts of viscosity reducing agent are placed in a vacuum environment, phosphate ester (purchased from BYK Chemical, brand BYK-W 9010) and high molecular weight copolymer alkyl ammonium salt (purchased from BYK Chemical, brand BYK-9076) are selected in a weight ratio of 1:1 as the viscosity reducing agent, the weight ratio of the prepolymer to the second thermal conductive filler is 3:7, the weight percentage of the viscosity reducing agent in component B is 0.6%, and the mixture is stirred at room temperature until it is uniformly mixed to obtain component B;

[0044] S3. When in use, the prepared component A and component B are uniformly mixed in a volume ratio of 1:1 to obtain a two-component polyurethane thermal conductive structural adhesive.

[0045] Example 2

[0046] A two-component polyurethane thermal conductive adhesive is different from Example 1 in that: in step S1, 100 parts of polyether polyol and 200 parts of castor oil modified polyol are uniformly mixed so that the weight ratio of polyether polyol to castor oil modified polyol is 1:2.

[0047] Example 3

[0048] A two-component polyurethane thermal conductive structural adhesive is different from Example 1 in that: in step S1, the castor oil modified polyol selected is produced by Ito Oil Manufacturing Co., Ltd., with the brand AC-009 (aromatic modified castor oil polyol); 100 parts of polyether polyol and 300 parts of castor oil modified polyol are uniformly mixed so that the weight ratio of polyether polyol to castor oil modified polyol is 1:3.

[0049] Example 4

[0050] A two-component polyurethane thermal conductive structural adhesive, which is different from Example 1 in that: in step S1, the castor oil modified polyol selected and the modified castor oil selected in step S2 are both a mixture of AC-009 produced by Ito Oil Manufacturing Co., Ltd. and A-4100 (aliphatic modified castor oil polyol) produced by Shanghai Jingri New Material Technology Co., Ltd. in a weight ratio of 1:1; in step S2, 100 parts of isocyanate and 27.5 parts of modified castor oil are mixed and reacted so that the weight ratio of isocyanate to modified castor oil is 10:2.75.

[0051] Example 5

[0052] A two-component polyurethane thermal conductive structural adhesive, which is different from Example 1 in that: in step S1, the castor oil modified polyol selected is BP-19 (aromatic modified castor oil polyol) produced by Shanghai Benyou New Material Technology Co., Ltd., and 100 parts of polyether polyol and 300 parts of castor oil modified polyol are mixed so that the weight ratio of polyether polyol to castor oil modified polyol is 1:3;.

[0053] Example 6

[0054] A two-component polyurethane thermal conductive structural adhesive is different from Example 1 in that: in step S1, the castor oil modified polyol selected is a mixture of BP-19 and BP-09 (aromatic modified castor oil polyol) produced by Shanghai Benyou New Material Technology Co., Ltd. in a weight ratio of 1:1, and 100 parts of polyether polyol and 200 parts of castor oil modified polyol are uniformly mixed so that the weight ratio of polyether polyol to castor oil modified polyol is 1:2; in step S2, the isocyanate selected is MDI-50 produced by Wanhua Chemical Group Co., Ltd.

[0055] Example 7

[0056] A two-component polyurethane thermally conductive structural adhesive, which is different from Example 1 in that: in step 1, the castor oil modified polyol selected is a mixture of H-52 (aliphatic modified castor oil polyol) produced by Ito Oil Manufacturing Co., Ltd. and BP-19 produced by Shanghai Benyou New Materials Technology Co., Ltd. in a weight ratio of 1:1, and 100 parts of polyether polyol and 200 parts of castor oil modified polyol are uniformly mixed so that the weight ratio of polyether polyol to castor oil modified polyol is 1:2; in step S2, the isocyanate selected is MDI-50 produced by Wanhua Chemical Group Co., Ltd.

[0057] It is worth noting that the above embodiments are only a few specific embodiments of the technical solution of the present application and should not be considered as limiting the scope of protection of the present application.

[0058] For example, in other embodiments, the polyether polyol in step S1 can also be selected from conventional commercial products, as long as the number average molecular weight of the polyether polyol is 500-2000 and the functionality is 3. In some embodiments, the molecular weight of the polyether polyol is any one of 500 (available from Bluestar Dongda Chemical Co., Ltd., with the brand name MN-500) and 700 (available from Bluestar Dongda Chemical Co., Ltd., with the brand name MN-700).

[0059] In other embodiments, the castor oil-modified polyol in step S1 can be selected from one or a mixture of aromatic modified castor oil polyol and aliphatic modified castor oil polyol. Specifically, the castor oil-modified polyol can be selected from one or more mixtures of H-30, H-31, H-52, H-368, AC-008 and AC-009 produced by Ito Oil Manufacturing Co., Ltd., A-21 and A-4100 produced by Shanghai Jingri New Material Technology Co., Ltd., and BP-09 and BP-19 produced by Shanghai Benyou New Material Technology Co., Ltd.

[0060] In other embodiments, the particle size of the first small-particle aluminum hydroxide in the first thermally conductive filler in step S1 is ≤15 μm, and the particle size of the first large-particle aluminum hydroxide is ≥20 μm and ≤50 μm. The two-component polyurethane thermally conductive structural adhesive made using aluminum hydroxide within these particle size ranges can achieve a higher filling amount and realize excellent thermal conductive flame retardant effects.

[0061] Preferably, the particle size of the first small-size aluminum hydroxide is 5 μm or 8 μm, and the particle size of the first large-size aluminum hydroxide is 20 μm or 50 μm; any one of 5 μm aluminum hydroxide and 20 μm aluminum hydroxide, 8 μm and 20 μm, 8 μm and 50 μm, 20 μm and 50 μm, and 5 μm and 50 μm in the first thermal conductive filler is a preferred embodiment. When the total content of aluminum hydroxide remains unchanged, adjusting the particle size combination has no significant effect on the overall flame retardant properties of the product.

[0062] In other embodiments, the weight ratio of the first small-particle aluminum hydroxide and the first large-particle aluminum hydroxide in the first thermally conductive filler of step S1 can be any weight ratio in the range of 1:(1-5). The two-component polyurethane thermally conductive structural adhesive prepared using the first thermally conductive filler within this weight ratio range can achieve good thermal conductivity and flame retardant effects.

[0063] In other embodiments, the weight ratio of the polyether polyol to the castor oil-modified polyol in step S1 can be any weight ratio within the range of 1:(1-3), and the performance of the two-component polyurethane thermal conductive structural adhesive prepared using any ratio within this weight ratio range is within an acceptable range.

[0064] In other embodiments, the weight ratio of the polyol composition and the first thermally conductive filler in step S1 can be any weight ratio within 1:(1-2); further, the weight ratio of the polyol composition and the first thermally conductive filler is 7:(10-14); the performance of the two-component polyurethane thermally conductive structural adhesive prepared using any ratio within the above two weight ratio ranges is within an acceptable range.

[0065] In other embodiments, the isocyanate in step S2 can be any one of CDMDI-100L, MDI-50 and MDI-100 produced by Wanhua Chemical Group Co., Ltd., which has no significant effect on the main improvement of the relevant mechanical properties of the present application.

[0066] In other embodiments, the modified castor oil in step S2 can be selected from one or a mixture of aromatic modified castor oil polyols and aliphatic modified castor oil polyols. Specifically, the modified castor oil can be selected from one or more mixtures of H-30, H-31, H-52, H-368, AC-008 and AC-009 produced by Ito Oil Manufacturing Co., Ltd., A-21 and A-4100 produced by Shanghai Jingri New Material Technology Co., Ltd., and BP-09 and BP-19 produced by Shanghai Benyou New Material Technology Co., Ltd.

[0067] In other embodiments, the particle size of the second smallest particle size aluminum hydroxide in the second thermally conductive filler in step S2 is ≤15 μm, and the particle size of the second largest particle size aluminum hydroxide is ≥20 μm and ≤50 μm. The two-component polyurethane thermally conductive structural adhesive made using aluminum hydroxide within these particle size ranges can achieve a higher filling amount and achieve excellent thermal conductive flame retardant effects. The second thermally conductive filler uses 5 μm aluminum hydroxide with 20 μm aluminum hydroxide, 8 μm with 20 μm, 8 μm with 50 μm, 20 μm with 50 μm, and 5 microns with 50 microns. Any one of these is a preferred embodiment. When the total content of aluminum hydroxide remains unchanged, adjusting the particle size combination has no significant effect on the overall flame retardant properties of the product.

[0068] In other embodiments, the weight ratio of the second smallest particle size aluminum hydroxide and the second largest particle size aluminum hydroxide in the second thermally conductive filler of step S2 can be any weight ratio in the range of 1:(1-5). The two-component polyurethane thermally conductive structural adhesive prepared using the second thermally conductive filler within this weight ratio range can achieve good thermal conductivity and flame retardant effects.

[0069] In other embodiments, the viscosity reducing agent in step S2 can also be a high molecular weight copolymer alkylamine salt, wherein the high molecular weight alkylammonium salt is a mixture of a reaction product of a special polymer and 2-ethylhexyl acrylate, and a polyethylene polypropylene glycol monobutyl ether phosphate compound; the special polymer is a polymer of ethylenediamine and ethyleneimine. In some embodiments, the viscosity reducing agent is BYK-W 9010, BYK-W9076, or a mixture of BYK-W 9010 and BYK-W9076 in any weight ratio.

[0070] In other embodiments, the weight ratio of isocyanate to modified castor oil in step S2 can be any ratio within the range of 10:(2-4).

[0071] In other embodiments, when preparing the prepolymer in step S2, the isocyanate and the modified castor oil can be reacted in an environment of 50-80° C. for 1-3 hours, wherein the temperature conditions, reaction time and whether to stir are adaptive adjustments made according to the initial viscosity and reaction rate of the materials, and all values ​​within this range are reasonable and feasible.

[0072] In other embodiments, the weight ratio of the prepolymer to the second thermally conductive filler in step S2 can be any weight ratio within the range of 3:(7-12), and the weight percentage of the viscosity reducing agent in component B can be any percentage within the range of 0.3-0.8%. In some embodiments, the weight percentage of the viscosity reducing agent in component B is any one of 0.4%, 0.5%, 0.6%, and 0.7%.

[0073] In other embodiments, in step S3, component A and component B can be mixed at any volume ratio within 1: (0.9-1.1), and the prepared two-component polyurethane thermal conductive structural adhesive can maintain good bonding performance and curing performance.

[0074] In other embodiments, a conventional catalyst is added to the two-component polyurethane thermally conductive structural adhesive based on the present application, which is also within the embodiment claimed for protection in the present application.

[0075] Comparative Example

[0076] Comparative Example 1: Debon 2028 structural adhesive (purchased from Yantai Debon Technology Co., Ltd., a two-component polyurethane thermal conductive structural adhesive with brand number 2028) which is currently widely used on the market, wherein the polyol adopts a castor oil system, and the thermal conductive filler comprises aluminum hydroxide, aluminum oxide and part of aluminum nitride.

[0077] Performance Testing

[0078] The two-component polyurethane thermal conductive structural adhesives in Examples 1-7 and Comparative Example 1 were subjected to the following tests, and the test items and test standards are as follows:

[0079] Thermal conductivity, unit: W / m·k, according to ASTM D5470;

[0080] Density, unit: g / cm 3 , according to GB / T 13354;

[0081] Elongation at break, unit: %, according to GB / T 528;

[0082] Tensile strength, unit: MPa, according to GB / T 528;

[0083] The thickness of the pure cured product when it reaches UL94-V0 grade, in mm;

[0084] The test results are shown in Table 1.

[0085] Table 1:

[0086]

[0087] By comparing Examples 1-7 with Comparative Example 1, it can be seen that the two-component polyurethane thermally conductive structural adhesive in the embodiment of the present application can reduce the density of the polyurethane product while maintaining the thermal conductivity when used, and can meet the demand for lightweight products; at the same time, aluminum hydroxide is added to components A and B as a thermally conductive filler, which can reach the UL94-V0 grade when the thickness is 1.5 mm, thus achieving the flame retardant requirement.

[0088] By comparing Examples 1-7 with Comparative Example 1 and combining with Table 1, it can be seen that castor oil-modified polyol is added to the components A and B of the polyurethane adhesive in the embodiment of the present invention, and the molecular weight of the polyether polyol in component A is relatively high, and the functionality is 3, so that the elongation at break of the product can be improved after the isocyanate, the polyether polyol and the castor oil-modified polyol are cured, thereby ensuring that the product has a certain toughness after the bonding is implemented, and ensuring that the product does not crack.

[0089] Adjusting the weight ratio of polyether polyol and castor oil modified polyol in component A within a certain range has no significant effect on the various indicators of the two-component polyurethane thermal conductive structural adhesive, which can achieve good thermal conductivity and flame retardant properties, and maintain good toughness and strength as well as low density.

[0090] By comparing Examples 1-7 and combining with Table 1, when the castor oil-modified polyol in component A of Example 4 and the modified castor oil in component B are both a mixture of AC-009 and A-4100 in a weight ratio of 1:1, it can be found that when the aromatic modified castor oil polyol and the aliphatic modified castor oil polyol are compounded, the tensile strength of the two-component polyurethane thermal conductive structural adhesive product is significantly improved, the elongation at break is slightly decreased, and the overall performance is better.

[0091] Combined with Examples 6-7, when the castor oil-modified polyol in component A is compounded with aromatic modified castor oil polyol H-52 and aliphatic modified castor oil polyol BP-19, and component B only uses aromatic modified castor oil polyol H-368, it can be seen that the thermal conductivity, density and elongation at break of the product can be slightly improved.

[0092] By selecting fillers in components A and B, matching the particle sizes of the selected fillers, selecting a polyol composition, and compounding a viscosity reducing agent, the present application can add a large amount of aluminum hydroxide to the base resin while controlling the product density and meeting the thermal conductivity requirements, thereby improving the flame retardancy of the product, maintaining or even improving the tensile strength and elongation at break of the product, overcoming the risk of cracking caused by the large amount of inorganic fillers added, and having excellent application performance.

[0093] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed, but such modifications are protected by patent law as long as they are within the scope of the claims of the present application.

Claims

1. A two-component polyurethane thermal conductive structural adhesive, It is characterized in that It includes component A and component B in a volume ratio of 1:(0.9-1.1); The A component includes a polyol composition and a first thermally conductive filler in a weight ratio of 1:(1-2); Wherein, the polyol composition comprises polyether polyol and castor oil modified polyol in a weight ratio of 1:(1-3); The B component includes a prepolymer and a second thermally conductive filler in a weight ratio of 3:(7-12); The first thermally conductive filler and the second thermally conductive filler are both aluminum hydroxide; The B component also includes 0.3-0.8 wt % of a viscosity reducing agent.

2. The two-component polyurethane thermal conductive structural adhesive according to claim 1, It is characterized in that The viscosity reducing agent is one or more combinations of phosphate ester and high molecular weight copolymer alkyl ammonium salt.

3. The two-component polyurethane thermal conductive structural adhesive according to claim 1, It is characterized in that The first thermally conductive filler and the second thermally conductive filler both include two types of aluminum hydroxide with different particle sizes.

4. The two-component polyurethane thermal conductive structural adhesive according to claim 3, It is characterized in that The first thermally conductive filler comprises a first small-particle aluminum hydroxide and a first large-particle aluminum hydroxide, and a weight ratio of the first small-particle aluminum hydroxide to the first large-particle aluminum hydroxide is 1:(1-5); The second thermally conductive filler comprises a second small-particle aluminum hydroxide and a second large-particle aluminum hydroxide, and a weight ratio of the second small-particle aluminum hydroxide to the second large-particle aluminum hydroxide is 1:(1-5); Wherein, the particle sizes of the first small-particle aluminum hydroxide and the second small-particle aluminum hydroxide are both ≤15 μm; The particle sizes of the first large particle size aluminum hydroxide and the second large particle size aluminum hydroxide are both ≥20 μm and ≤50 μm.

5. The two-component polyurethane thermal conductive structural adhesive according to claim 4, It is characterized in that The particle size of the first small-particle aluminum hydroxide is 5 μm or 8 μm; The particle size of the second small-particle aluminum hydroxide is 5 μm or 8 μm; The particle size of the first largest particle size aluminum hydroxide is 20 μm or 50 μm; The particle size of the second largest particle size aluminum hydroxide is 20 μm or 50 μm.

6. The two-component polyurethane thermal conductive structural adhesive according to claim 1, It is characterized in that The weight ratio of the polyol composition to the first thermally conductive filler is 7:(10-14).

7. The two-component polyurethane thermal conductive structural adhesive according to claim 1, It is characterized in that The weight ratio of the polyether polyol to the castor oil modified polyol is 1:

3.

8. The two-component polyurethane thermal conductive structural adhesive according to claim 1, It is characterized in that The number average molecular weight of the polyether polyol is 500-2000 and the functionality is 3.

9. The two-component polyurethane thermal conductive structural adhesive according to claim 1, It is characterized in that The prepolymer is formed by prepolymerization of isocyanate and modified castor oil, wherein the weight ratio of the isocyanate to the modified castor oil is 10:(2-4).

10. The two-component polyurethane thermal conductive structural adhesive according to claim 9, It is characterized in that The preparation method of the prepolymer is as follows: placing the isocyanate and the modified castor oil at 50-80° C. and reacting for 1-3 hours to obtain the prepolymer.

11. The two-component polyurethane thermal conductive structural adhesive according to claim 9, It is characterized in that The weight ratio of the isocyanate to the modified castor oil is 10:2.

75.

12. The two-component polyurethane thermal conductive structural adhesive according to claim 9, It is characterized in that The modified castor oil comprises one or a combination of aliphatic modified castor oil polyol and aromatic modified castor oil polyol.

13. The two-component polyurethane thermal conductive structural adhesive according to claim 1, It is characterized in that The castor oil modified polyol comprises one or a combination of aliphatic modified castor oil polyol and aromatic modified castor oil polyol.

14. A method for preparing a two-component polyurethane thermally conductive structural adhesive according to any one of claims 1 to 13, It is characterized in that The following steps are involved: preparing the A component; preparing the B component; The A component and the B component are mixed in a volume ratio of 1:(0.9-1.1).

Citation Information

Cited By

  • Non‑silicone thermal pad and preparation method therefor

    WO2026123586A1